Silicon carbide ceramic
Selecting SiC ceramics by manufacturing route, residual phases, named grade, test conditions and component requirements.
Tags: materials, ceramics, silicon-carbide
Research draft — not customer-confirmed
On this page
Silicon carbide (SiC) ceramics serve in wear parts, seals, furnace components and semiconductor equipment, but the material name does not identify one composition or property set. Manufacturing route, residual phases, porosity, graphite additions and electrical grade can change the selection substantially. Specify the manufacturer's complete grade and supplied condition rather than ordering an interchangeable generic SiC part.
Identify the ceramic family
Schunk distinguishes recrystallized SiC, sintered SiC, reaction-bonded/metal-matrix-bonded SiC, silicon-nitride-bonded SiC and oxide-bonded SiC. These have different densities and porosities. Thus, a porous kiln-furniture material and a dense seal-face material should not share a property table merely because both contain silicon carbide. Identify whether the requirement concerns a bulk ceramic, a coating or a particular composite structure. Schunk, Silicon Carbide in Comparison
CeramTec's ROCAR brochure explains two important routes. Reaction-bonded SiC, RBSiC/SiSiC, involves silicon infiltration into an SiC matrix, creating additional SiC while leaving a silicon-containing material. Low firing shrinkage facilitates large or complex components. Sintered SiC, SSiC, is densified by high-temperature sintering, with substantially different shrinkage and residual-phase characteristics. These routes are not alternative labels for the same finished material. CeramTec, ROCAR silicon carbide brochure
CoorsTek's brochure, carrying a printed ©2024 / 01024 J footer, describes its reaction-bonded material as retaining approximately 10% metallic silicon. It separately describes direct-sintered material above 99% purity and PureSiC CVD material above 99.9995% purity. These are specific product-family statements, not universal percentages for every reaction-bonded, sintered or CVD product. Its charts are typical and explicitly depend on manufacturing method, part size and shape. CoorsTek, Silicon Carbides
Purity and electrical behavior need their own requirements
Morgan's Performance SiC sheet, with a printed 2013 copyright, reports 99.9995% purity by GDMS and identifies high-resistivity and extremely-low-resistivity variants. Its typical electrical-resistivity entries at 20 °C, measured by the Van der Pauw method, are greater than 1 Ω·cm for Performance SiC and less than 0.1 Ω·cm for Performance ELR SiC.
Specify resistivity and critical impurities separately; a headline purity percentage does not resolve both. Morgan Advanced Materials, Performance SiC datasheet
Compare properties on matched test bases
The Morgan sheet also illustrates why temperature belongs beside a strength value:
| Typical property | Named material and test basis | Result |
|---|---|---|
| Flexural strength | Performance SiC; ASTM C1161; 20 °C | 370 MPa |
| Flexural strength | Performance SiC; ASTM C1161; 1,300 °C | 560 MPa |
These variable typical results establish neither component tensile allowables nor continuous service at 1,300 °C. Preserve specimen, surface, statistical and environmental conditions. Morgan, Performance SiC mechanical data
A different bounded example is CeramTec's ROCAR 3D SiSiC sheet. It lists standard ROCAR 3D density 2.94 g/cm³, calculated silicon content approximately 24 mass%, and 180 MPa four-point bending strength according to DIN EN 843-1. The separate 3D light column lists 2.88 g/cm³, approximately 31 mass% silicon and 160 MPa. Those columns must not be combined into a fictitious best-of-both material.
The sheet warns that sample values cannot be transferred to arbitrary component formats or surface qualities. It also lists standard ROCAR 3D expansion coefficients of 3.9, 4.3 and 4.7 × 10⁻⁶/K over 30–400, 30–600 and 30–1,000 °C, respectively. “Low expansion” therefore does not mean zero expansion or a coefficient independent of temperature interval. No printed revision date is assigned to this undated sheet. CeramTec, ROCAR 3D material data
Match thermal and chemical exposure to the grade
CeramTec's ROCAR brochure places a 1,350 °C operating-temperature limit on its silicon-containing reaction-bonded family and describes a chemical-resistance limitation up to pH 10. Treat those as that brochure's bounded family guidance, not general SiC ratings. They do not resolve the effects of a particular chemical species, concentration, atmosphere, pressure or exposure time. Confirm the actual medium and grade with the component supplier. CeramTec, reaction-bonded ROCAR guidance
Schunk separately identifies CarSIK-NG as silicon-nitride-bonded SiC for particular kiln-furniture applications and describes use in an oxidative environment. Its published application-temperature statement belongs to that grade and use context. It must not be transferred to a dense seal, another binder system or a different furnace atmosphere. Schunk, bonded SiC families and applications
For thermal cycling, specify ramp rates, local heat flux, cooling medium, wall thickness, constraints and cycle count. High thermal conductivity and low expansion are useful selection inputs; neither establishes a universal safe quench or thermal-shock temperature difference for the finished part.
Seal and wear performance is a system property
Morgan's seals-and-bearings brochure, printed ©03/2020 v1, distinguishes monolithic reaction-bonded SiC, graphite-containing reaction-bonded composites, sintered SiC and graphite-loaded sintered grades. It relates their behavior to mating materials and lubrication, including improved marginal-lubrication or dry-run survivability for particular graphite-containing options. Such comparisons do not establish indefinite dry-running capability or a universal pressure–velocity limit.
Select the counterface, process fluid, lubrication regime, start/stop duty, solids, speed and load together with the ceramic grade. Define the surface finish, flatness and wear/leakage acceptance criteria on the actual seal or bearing assembly. Morgan, Silicon Carbide Materials for Seals & Bearings
Specify the finished component
Agree the manufacturing and finishing route before freezing the drawing. Identify near-net geometry, machining allowance, critical surfaces, edges, holes and joining/mounting interfaces. Require the supplier to assess geometry and surface quality against the selected material and process rather than assuming that a small test bar represents every shape.
For acceptance, retain grade, batch identity, manufacturing route, residual-phase or purity requirements, density/porosity basis, dimensions and specified tests. Separate supplier typical values from contractual limits and approved design values. Temperature, strength, electrical and chemical requirements should each retain their own test and service conditions. A change from sintered to reaction-bonded material, or between electrical CVD grades, requires a complete requirements comparison rather than substitution by the SiC name alone.