Morgan reports typical flexural strength of **370 MPa at 20°C** and **560 MPa at 1,300°C** for **CVD Performance SiC**. Morgan prints ASTM C1161 beside the flexural entry. [ASTM scopes C1161 to ambient temperature](https://store.astm.org/c1161-18.html), so confirm the 1,300°C procedure with Morgan before comparing methods. Establish tensile allowables and hot-service limits separately. [Morgan Performance SiC mechanical data](https://www.morganthermalceramics.com/media/4w2fxqma/performance-sic.pdf)

## Identify the ceramic family

Schunk distinguishes recrystallized SiC, sintered SiC, reaction-bonded/metal-matrix-bonded SiC, silicon-nitride-bonded SiC and oxide-bonded SiC. These have different densities and porosities. Thus, a porous kiln-furniture material and a dense seal-face material should not share a property table merely because both contain silicon carbide. Identify whether the requirement concerns a bulk ceramic, a coating or a particular composite structure. [Schunk, Silicon Carbide in Comparison](https://www.schunk-group.com/technical-ceramics/en/materials/silicon-carbide)

CeramTec's ROCAR brochure explains two important routes. **Reaction-bonded SiC, RBSiC/SiSiC**, involves silicon infiltration into an SiC matrix, creating additional SiC while leaving a silicon-containing material. Low firing shrinkage facilitates large or complex components. **Sintered SiC, SSiC**, is densified by high-temperature sintering, with substantially different shrinkage and residual-phase characteristics. These routes are not alternative labels for the same finished material. [CeramTec, ROCAR silicon carbide brochure](https://www.ceramtec-group.com/fileadmin/user_upload/Corporate/11_Downloads/09_Pumps-Valves-Seals/cz_rocar_en.pdf)

CoorsTek's brochure, carrying a printed **©2024 / 01024 J** footer, describes its reaction-bonded material as retaining approximately **10% metallic silicon**. It separately describes direct-sintered material above **99% purity** and PureSiC CVD material above **99.9995% purity**. These are specific product-family statements, not universal percentages for every reaction-bonded, sintered or CVD product. Its charts are typical and explicitly depend on manufacturing method, part size and shape. [CoorsTek, Silicon Carbides](https://www.coorstek.com/media/4249/silicon-carbides.pdf)

## Purity and electrical behavior need their own requirements

Morgan's **Performance SiC** sheet, with a printed **2013 copyright**, reports **99.9995% purity by GDMS** and identifies high-resistivity and extremely-low-resistivity variants. Its typical electrical-resistivity entries at **20 °C**, measured by the **Van der Pauw** method, are **greater than 1 Ω·cm** for Performance SiC and **less than 0.1 Ω·cm** for Performance ELR SiC.

Specify resistivity and critical impurities separately; a headline purity percentage does not resolve both. [Morgan Advanced Materials, Performance SiC datasheet](https://www.morganthermalceramics.com/media/4w2fxqma/performance-sic.pdf)

## Compare properties on matched test bases

Morgan lists ASTM C1161 alongside its flexural data. The standard covers ambient testing. Ask Morgan which procedure it used for the elevated-temperature result.

| Typical property | Named material and test basis | Result |
| --- | --- | ---: |
| Flexural strength | Performance SiC; ASTM C1161; 20 °C | 370 MPa |
| Flexural strength | Performance SiC; 1,300 °C; confirm the test procedure | 560 MPa |

These variable typical results establish neither component tensile allowables nor continuous service at 1,300 °C. Preserve specimen, surface, statistical and environmental conditions. [Morgan, Performance SiC mechanical data](https://www.morganthermalceramics.com/media/4w2fxqma/performance-sic.pdf)

A different bounded example is CeramTec's **ROCAR 3D SiSiC** sheet. It lists standard ROCAR 3D density **2.94 g/cm³**, calculated silicon content approximately **24 mass%**, and **180 MPa four-point bending strength according to DIN EN 843-1**. The separate **3D light** column lists **2.88 g/cm³**, approximately **31 mass% silicon** and **160 MPa**. Those columns must not be combined into a fictitious best-of-both material.

The sheet warns that sample values cannot be transferred to arbitrary component formats or surface qualities. It also lists standard ROCAR 3D expansion coefficients of **3.9, 4.3 and 4.7 × 10⁻⁶/K** over **30–400, 30–600 and 30–1,000 °C**, respectively. “Low expansion” therefore does not mean zero expansion or a coefficient independent of temperature interval. No printed revision date is assigned to this undated sheet. [CeramTec, ROCAR 3D material data](https://www.ceramtec-group.com/fileadmin/user_upload/Corporate/11_Downloads/15_Various_Industrial_Applications/Datasheet_CeramTec_3D-Printing_SiSC.pdf)

## Match thermal and chemical exposure to the grade

CeramTec's ROCAR brochure places a **1,350 °C** operating-temperature limit on its silicon-containing reaction-bonded family and describes a chemical-resistance limitation up to **pH 10**. Treat those as that brochure's bounded family guidance, not general SiC ratings. They do not resolve the effects of a particular chemical species, concentration, atmosphere, pressure or exposure time. Confirm the actual medium and grade with the component supplier. [CeramTec, reaction-bonded ROCAR guidance](https://www.ceramtec-group.com/fileadmin/user_upload/Corporate/11_Downloads/09_Pumps-Valves-Seals/cz_rocar_en.pdf)

Schunk separately identifies **CarSIK-NG** as silicon-nitride-bonded SiC for particular kiln-furniture applications and describes use in an oxidative environment. Its published application-temperature statement belongs to that grade and use context. It must not be transferred to a dense seal, another binder system or a different furnace atmosphere. [Schunk, bonded SiC families and applications](https://www.schunk-group.com/technical-ceramics/en/materials/silicon-carbide)

For thermal cycling, specify ramp rates, local heat flux, cooling medium, wall thickness, constraints and cycle count. High thermal conductivity and low expansion are useful selection inputs; neither establishes a universal safe quench or thermal-shock temperature difference for the finished part.

## Seal and wear performance is a system property

Morgan's seals-and-bearings brochure, printed **©03/2020 v1**, distinguishes monolithic reaction-bonded SiC, graphite-containing reaction-bonded composites, sintered SiC and graphite-loaded sintered grades. It relates their behavior to mating materials and lubrication, including improved marginal-lubrication or dry-run survivability for particular graphite-containing options. Such comparisons do not establish indefinite dry-running capability or a universal pressure–velocity limit.

Select the counterface, process fluid, lubrication regime, start/stop duty, solids, speed and load together with the ceramic grade. Define the surface finish, flatness and wear/leakage acceptance criteria on the actual seal or bearing assembly. [Morgan, Silicon Carbide Materials for Seals & Bearings](https://www.morganthermalceramics.com/media/ivect4ml/morgan-seals-bearings-silicon-carbide.pdf)

## Specify the finished component

Agree the manufacturing and finishing route before freezing the drawing. Identify near-net geometry, machining allowance, critical surfaces, edges, holes and joining/mounting interfaces. Require the supplier to assess geometry and surface quality against the selected material and process rather than assuming that a small test bar represents every shape.

For acceptance, retain grade, batch identity, manufacturing route, residual-phase or purity requirements, density/porosity basis, dimensions and specified tests. Separate supplier typical values from contractual limits and approved design values. Temperature, strength, electrical and chemical requirements should each retain their own test and service conditions. A change from sintered to reaction-bonded material, or between electrical CVD grades, requires a complete requirements comparison rather than substitution by the SiC name alone.