Skip to content
PlanarManufacturing Wiki

TPU

Thermoplastic polyurethane selection by chemistry, grade, processing route and test conditions.

Tags: materials, polymers, elastomers

Research draft — not customer-confirmed

On this page

Identity and selection scope

TPU means thermoplastic polyurethane, an elastic polymer processed using thermoplastic manufacturing methods. BASF identifies injection molding, extrusion, calendering and blow molding among the processes for its Elastollan TPU products, and supplies special grades and masterbatches for different applications. A family name or hardness rating is therefore insufficient to specify a component. BASF: Elastollan TPU overview

Record the manufacturer, complete grade and suffix, color/additive package, supplied form and manufacturing route. Keep pellets, extrusion profiles, filament, powder and finished parts distinct. Replacing a molded component with a printed one requires evidence for that new route, even when both materials carry the same nominal Shore hardness. TPU processing instructions also cannot replace the mixing and cure requirements of a reactive cast-polyurethane system.

Chemistry and exposure

Lubrizol's TPU extrusion guide distinguishes polyether- and polyester-based materials. It describes polyether grades as a usual choice where hydrolytic stability, low-temperature flexibility or fungal resistance matters, while noting that additive compounding can improve polyester grades' hydrolysis and fungal resistance. This supports selecting a particular formulation; it does not establish an unconditional ranking or a universal water-service limit. Lubrizol: TPU extrusion processing guide

For qualification, state the exact fluid, concentration, temperature, exposure time and strain. Include cleaning and disinfection cycles, lubricants, outdoor exposure and thermal excursions where relevant. Ask for retained tensile, tear, compression or dimensional performance against an explicit acceptance limit. A description such as “oil resistant” does not identify the oil formulation or show that an assembled seal will retain its function.

A named-grade property example

Covestro describes Desmopan 3385A as an extrusion and injection-molding grade. Its current product page lists typical mechanical properties under 23 °C/50% relative humidity:

Property Typical value and method
Shore A hardness 85, DIN ISO 7619-1, 1-second reading
Shore D hardness 33, same method and reading time
Ultimate tensile strength 52 MPa, DIN 53504, 200 mm/min
Stress at 100% strain 5.8 MPa, DIN 53504, 200 mm/min
Compression set 42%, DIN ISO 815-1 Method A, 24 hours at 70 °C

Source: Covestro: Desmopan 3385A typical values.

The two hardness scales are separate measurements, not percentages or a linear conversion. Stress at 100% strain is not Young's modulus and is not an allowable sustained working stress. Preserve test speed, temperature, humidity and method when comparing these values. The web table does not supply a complete specimen-conditioning history or a printed revision date; obtain the applicable controlled datasheet for contractual use.

For a flexible pad or mount, specify the load-deflection behavior and recovery needed in the actual geometry. For a roller or repeatedly flexed part, include cyclic heating, frequency, strain amplitude and fatigue testing. Tensile strength alone does not settle those requirements.

Drying and material handling before processing

BASF's Elastollan processing brochure carries a September 2019 note. It warns that excess granulate moisture can cause foaming, melt bubbles, extrusion throughput variation and poor finished-product quality. Its general guidance targets water content below 0.02%, with drying conditions differentiated by product family and hardness and an instruction to consult the specific product information. That target is a processing recommendation for the covered materials, not a specification for equilibrium moisture in a finished component. BASF: processing recommendations

The brochure also applies drying requirements to masterbatches and other additives. Qualify the dryer, starting material condition and transfer to the processing machine, rather than treating a fixed oven duration as proof of dryness. Keep processing moisture control separate from post-production conditioning and the temperature/humidity at final inspection. BASF: drying guidance

Route-specific manufacturing controls

Lubrizol requires product-specific barrel and die settings and notes that extrusion rate affects quality. It also warns that masterbatch and regrind need drying and can materially affect the product. Its guidance is based on laboratory work and does not itself establish end-product performance. Retain grade, additions, material history and extrusion settings when qualifying a profile or tube. Lubrizol: extrusion controls

For injection molding, verify filling, weld lines, shrinkage, demolding damage and dimensions using the actual tool and process. For extrusion, include profile uniformity, wall thickness, cooling and downstream tension. A processing-temperature setting describes manufacturing; it is not a continuous service-temperature rating.

EOS's manufacturer-hosted TPU 1301 data document, marked last change 14 March 2022, explicitly warns that additively manufactured properties depend on build direction, system, layer thickness and powder preparation. Its historical table lists ISO 527 tensile strength of 7 MPa in X/Y and 5 MPa in Z. These values illustrate why orientation must be recorded; they are not current universal TPU-printing allowables and cannot be substituted for injection-molded data. EOS: TPU 1301 historical data document

For a printed part, obtain the current material-and-machine parameter set, build orientation, powder or filament handling requirements and post-processing instructions. Test representative part features, including thin sections and connections, instead of relying only on a nominal infill percentage or a bulk-resin coupon.

Handling and finished-part validation

The German-market SDS for Desmopan 3385A 000000, version 3.1, is revised 21 September 2025 and printed 24 January 2026. It does not classify the supplied mixture under EU CLP, but still requires adequate ventilation and, where necessary, effective exhaust when opening fresh packaging, drying and processing; small emissions can occur under recommended conditions. The sheet separately addresses hot-melt contact. A room-temperature granulate classification does not describe every heated operation. Covestro: exact-grade SDS

A useful purchase and validation record includes:

  • Complete grade, chemistry, form, color and permitted additions or substitutions.
  • Property-source edition, test method, direction and conditioning history.
  • Drying and manufacturing records, including recycled-material history.
  • Actual load, motion, thermal cycle, fluids and cleaning sequence.
  • Finished-part dimensions, surface and internal-defect criteria.
  • Required aging, compression, abrasion, tear, fatigue or assembly tests.

Keep supplier typical data, contractual limits and measured component performance separate. Food-contact or medical suitability requires exact-grade documentation and intended-use conditions. The Lubrizol guide does not display a clear edition date; neither search-engine dates nor a website copyright establish its technical revision.

Material selection through production