# Louver forming tools

Cut-and-form louver tooling, single-hit and continuous versions, material-specific geometry limits, and sheet-motion clearance.

Reviewed: 2026-11-02

Tags: tooling, sheet-metal, forming, louvers

In CONIC's cited louver geometry, **1.5 mm** sheet gives height limits of **6.0 mm** for mild steel and **5.25 mm** for stainless steel and aluminum. A proposed **5 mm height and 12 mm width** also meets **width ≥ twice height**. At **5.5 mm** height, the stainless and aluminum limit is exceeded. Those checks cover the cited geometry only. Form direction, end spacing and clearance still matter. [CONIC technical sheet](https://www.conic.co.jp/en/tech/forming_tools/pdf/LOUVER_FOR_AIR_FLOW.pdf).

## Identity and feature geometry

Mate’s closed-end tool lances one side and raises the hood. The hood’s ends are closed and the front admits airflow. [Mate Technical Solutions Guide, revision E, 2021, printed p. 64](https://www.mate.com/wp-content/uploads/2021/03/LIT00682_TechSolutionsGuide_RevE_LR.pdf#page=66).

Specify length, opening height, hood width, radii and form direction.

Wilson Tool also describes louvers as sheet stops and offers a holder with replaceable size inserts. [Wilson Tool, louver applications](https://wilsontool.com/en-us/solutions/punching/eliminating-secondary-operations).

## Closed ends, open ends, and progressive length

Mate describes closed-end forms with rounded enclosed corners for exposed panels. Its open-end version adds end openings but exposes cut ends, favoring placement inside an enclosure. These are geometry and placement distinctions, not quantified airflow or load-capacity ratings. [Mate guide, printed p. 65](https://www.mate.com/wp-content/uploads/2021/03/LIT00682_TechSolutionsGuide_RevE_LR.pdf#page=67).

A single-hit tool and a continuous tool produce louvers differently. TRUMPF's cited catalog provides these particular examples for its listed punching and punch-laser machines. [TRUMPF punching-tools catalog, printed pp. 74–75](https://www.trumpf.com/filestorage/TRUMPF_Master/Products/Services/01_brochures/TRUMPF-punching-tools-catalog-EN.pdf#page=74).

| Catalog example | Tool action | Listed geometry | Listed sheet range |
| --- | --- | --- | --- |
| Single louver, complete tool 0699222 | Cuts and forms in one stroke | L × W × H = 60 × 12 × 5 mm | 0.8–2.5 mm |
| Continuous louver, complete tool 0699229 | Produces variable length by nibbling | W × H = 12 × 5 mm | 0.8–3.0 mm |

The continuous entry explicitly requires tooling designed for a particular sheet thickness. Its family range therefore does not mean one setup covers every thickness. Variable-length operation also remains bounded by machine travel, sheet handling, and the particular part layout. [TRUMPF, printed p. 75](https://www.trumpf.com/filestorage/TRUMPF_Master/Products/Services/01_brochures/TRUMPF-punching-tools-catalog-EN.pdf#page=75).

Mate's separate technique guidance describes starting continuous louvers at the center and working toward both ends in nominal 0.8 mm increments, with a possible center re-hit for flatness. This is a manufacturer's technique for the relevant tooling, not a universal feed increment for every progressive louver tool. [Mate forming techniques](https://www.mate.com/technical-resources/punch-press-resources/tips-techniques/forming/).

## Material and geometry conditions

CONIC's *Louver for Air Flow* sheet lists thickness up to 2.3 mm, width A at least twice height H, and height no greater than four thicknesses for mild steel or 3.5 thicknesses for stainless steel and aluminum. Its diagram also defines separate pitch and spacing conditions. These are requirements for the illustrated CONIC form and tooling, not generic louver limits. [CONIC technical sheet](https://www.conic.co.jp/en/tech/forming_tools/pdf/LOUVER_FOR_AIR_FLOW.pdf).

For an original example with `t = 1.5 mm`, those height comparisons give `4t = 6.0 mm` for mild steel and `3.5t = 5.25 mm` for the other listed categories. A proposed `H = 5 mm`, `A = 12 mm` satisfies both height comparisons and `A ≥ 2H`, because `12 ≥ 10 mm`. Raising H to 5.5 mm exceeds the stainless/aluminum height condition. Passing this arithmetic does not establish suitable material ductility, radii, spacing, tool capacity, or a successful production result. [CONIC](https://www.conic.co.jp/en/tech/forming_tools/pdf/LOUVER_FOR_AIR_FLOW.pdf).

## Direction, spacing, and machine clearance

Mate specifies a flat land of at least three thicknesses between adjacent louver fronts and backs, distinct from center pitch. Its 8 mm minimum end spacing concerns a different direction. [Mate guide, printed pp. 64–65](https://www.mate.com/wp-content/uploads/2021/03/LIT00682_TechSolutionsGuide_RevE_LR.pdf#page=66).

Form-down geometry can catch in dies, consume vertical clearance, or be flattened during later operations. Mate's general forming guidance favors making unavoidable form-down operations last. It also identifies corners of high louvers as vulnerable to splitting and describes grain orientation and forming lubricant as relevant to stressed forms. [Mate forming techniques](https://www.mate.com/technical-resources/punch-press-resources/tips-techniques/forming/).

A finished-feature envelope is consequently different from a collision-free sheet-motion envelope. Neighboring tools, existing forms, workholders, underside clearance, and the sheet's route through the machine can constrain a nested pattern even when its flat outlines do not overlap. This is an engineering implication of the forming-sequence guidance, not a universal keep-out dimension.

## Opening area is not airflow or strength

For a deliberately simplified geometric example, assume ten unobstructed rectangular front gaps, each 50 mm long and 3 mm high. Their summed front-opening area is `10 × 50 × 3 = 1,500 mm²`, or 15 cm². This is original arithmetic for the assumed apertures, not the hood's plan area or a manufacturer's effective free-area rating.

That area calculation does not predict flow rate, pressure drop, cooling, water exclusion, or structural strength. Actual rounded ends, side openings, screens, and flow direction can change the relevant passage geometry. Neither a forming-tool size nor a nominal opening area establishes a panel's mechanical load capacity. These are coverage limits of a tooling reference; performance requires the relevant design or test basis.

## Source dates and applicability

Mate's guide carries the actual footer LIT00682 Rev E 2021. The TRUMPF catalog's back-cover identifier is 1798794_EN_202204_S; the complete identifier is retained here rather than assigning an inferred issue date. CONIC's technical sheet and the cited Wilson Tool and Mate web pages do not establish technical issue dates in the inspected content. This article's reviewed date records its research review.

The cited sources do not establish a universal forming force, speed, tool life, tooling mount, or allowable height. Listed dimensions, thickness ranges, and techniques apply to the respective manufacturer's tooling and conditions; they do not establish a shop's installed machine capabilities or approved settings.

For broader tooling context, see [Sheet-metal tooling](index.md).