# Gravity die casting

Reusable-mold gravity casting, cores and thermal control, feeding and porosity, machining and material condition, and finished-part acceptance.

Reviewed: 2026-11-01

Tags: processes, shaping, casting

A hypothetical **12.0 kg pour** yields a **7.2 kg rough casting** after removing runners and feeders and a **6.0 kg finished component** after machining. That is **60% rough-casting yield** and **50% finished-part yield**. Match the delivered condition and yield boundary when comparing foundry quotations.

Gravity fills the reusable iron or steel mold. Specify the filling route, die opening and venting arrangement separately from pressure-assisted methods. [Foseco: gravity die casting](https://www.foseco.com/en/casting-processes/gravity-die-casting)

Haworth's **June 26, 2019** overview describes heating and coating the die, closing it, pouring, solidifying and removing the casting. Its process benefits are supplier capability descriptions, not a dimensional tolerance or mechanical-property guarantee for an arbitrary component. Identify the alloy, final condition, geometry and quantity before comparing the route with sand casting or machining. [Haworth: process overview](https://haworthcastings.co.uk/news/an-overview-of-gravity-die-casting)

## Reusable tooling and internal features

| Choice | Meaning for the manufacturing handoff |
| --- | --- |
| Reusable die surfaces | Define parting, opening direction, extraction and any moving tooling needed. |
| Metal core | Confirm that the core can withdraw without trapping the solidified component. |
| Expendable sand core | Define location, support, removal access and cleanliness of the resulting passage. |
| Machined internal feature | Allow stock and tool access in the agreed casting envelope. |

Foseco distinguishes permanent steel cores from resin-bonded sand cores; using expendable cores with a reusable die is a semi-permanent-mold route. Its discussion also notes that an impermeable die needs provision for venting. A reusable outside tool therefore does not establish that every internal feature is reusable, core-free or accessible after casting. [Foseco: cores and venting](https://www.foseco.com/en/casting-processes/gravity-die-casting)

Review finished and as-cast models together. Agree the parting line, draft, transitions, core interfaces, machining datums and retained stock. A critical hole position may depend on core location and subsequent machining; the external die dimensions alone do not define that relationship. Avoid freezing an undercut or enclosed passage before the foundry has confirmed extraction and removal.

## Filling, feeding and heat flow

Filling the cavity and feeding solidification shrinkage are separate tasks. Foseco describes runner/filter arrangements for controlling flow and risers at heavy sections for supplying liquid during solidification. A filled external shape does not prove that a thick junction is internally sound. [Foseco: filling and feeders](https://www.foseco.com/en/casting-processes/gravity-die-casting)

Ask the foundry to identify the relevant filling and feeding strategy, local thermal controls and the inspection stage used to qualify critical sections. Review thick-to-thin transitions, isolated masses and the surfaces that will be opened by machining. Adding more poured metal does not by itself prove that the liquid can feed the region that needs it.

Foseco's coating product guidance describes a deposited layer controlling heat transfer and release. Its DYCOTE formulations combine insulating and/or lubricating refractories with inorganic binders and serve gravity and low-pressure casting of identified non-ferrous alloys. Coating selection and application are process variables alongside the die, alloy and metal temperature. Do not treat die dressing as an incidental cosmetic operation or transfer a coating solely because both jobs use aluminum. [Foseco: permanent-mold coatings](https://www.foseco.com/en/products/die-coatings-for-permanent-mould-casting)

For a trial, record the approved die preparation, coating system and condition, thermal-control arrangement and production sequence. Compare first-off and steady production results. The same tool can operate in different thermal states; successful early samples do not automatically represent a full production run. The qualified route should define the actual controls rather than a universal die or pouring temperature.

## Porosity, machining and condition

Haworth's porosity guide distinguishes gas-related mechanisms from feeding/solidification problems and calls for identifying the mechanism before selecting corrective action. Its advice supports investigating melt, filling and thermal controls rather than prescribing one remedy for every pore seen in a machined surface. [Haworth: porosity and inspection planning](https://haworthcastings.co.uk/casting_guides/porosity-in-castings-causes-prevention-and-how-to-specify-inspection/)

Specify where internal discontinuities matter: a sealing wall, loaded boss and noncritical machining pad can require different evidence. Define inspection coverage and acceptance levels for the intended use. A surface examination, internal examination and leak test address different questions. A passing pressure test is not a universal measure of local fatigue or tensile behavior.

Separate material designation from final temper and processing. Agree whether heat treatment, straightening, machining, cleaning, surface treatment or any permitted impregnation forms part of the delivery. Confirm how those operations affect dimensions and which inspections occur afterward. Reworking a leak or removing a visible defect requires an agreed route; it should not be inferred from an otherwise acceptable alloy certificate.

## Scoped specification example

**ASTM B108/B108M-25** covers aluminum-alloy permanent-mold castings. ASTM's publisher page lists it as active and records **January 7, 2026** as its last update; that web-page update is distinct from the edition suffix. Its scope is for general-purpose applications and explicitly warns that it may not address all mechanical-property, integrity-test and verification needs of highly loaded or safety-critical applications. [ASTM: B108/B108M-25 public scope](https://store.astm.org/b0108_b0108m-25.html)

The public abstract distinguishes separately cast specimens from specimens taken from castings and relates specimen processing to the represented heat-treated condition. Do not describe a separate test bar as a measurement of every local section. The ordered grade, temper, specimen basis and additional component requirements must be explicit. The public summary establishes scope; use the applicable standard and purchase requirements for detailed acceptance. [Same specification: abstract](https://store.astm.org/b0108_b0108m-25.html)

## Original metal-yield budget

Assume a hypothetical pour uses **12.0 kg** of metal and produces a **7.2 kg** rough casting after removing runners/feeders. Subsequent machining removes **1.2 kg**, leaving a **6.0 kg** accepted component. Ignore oxidation, spillage, rejected castings and other losses.

| Quantity | Calculation | Result |
| --- | --- | --- |
| Rough-casting yield | 7.2 / 12.0 | 60% |
| Finished-part yield from poured metal | 6.0 / 12.0 | 50% |
| Runner/feeder return | 12.0 − 7.2 | 4.8 kg |
| Machining removal | 7.2 − 6.0 | 1.2 kg |
| Mass balance | 6.0 + 1.2 + 4.8 | 12.0 kg |

Thus a quoted 60% casting yield is not a 60% finished-part yield in this example. Returning the 4.8 kg for remelting does not make it free of processing cost or energy demand. These invented values do not predict a foundry's practical yield, remelt losses or acceptance rate. Compare quotations using the same yield boundary and delivered condition.

## Release and inspection handoff

Provide four groups of information:

1. **Final definition:** drawing/model revision, datums, dimensions, minimum walls, surface requirements and functional regions.
2. **Material and condition:** alloy specification/edition, temper, thermal processing, specimen basis and traceability.
3. **Manufacturing route:** die/core arrangement, agreed casting envelope, machining stock, secondary operations and permitted repair/removal routes.
4. **Acceptance:** examination type, coverage and limits, dimensional stage, any pressure/leak conditions, sampling and required records.

Haworth's **December 4, 2014** inspection overview distinguishes radiographic examination for internal features from dye-penetrant examination for surface flaws. Select methods for the actual geometry and specified discontinuities; neither a good-looking exterior nor a process name proves finished-part acceptance. [Haworth: testing and inspection](https://haworthcastings.co.uk/news/casting-testing-and-inspection/)

The Foseco and live Haworth guidance pages have no separately verified issue date here, apart from the dated 2019 process overview and 2014 inspection article. No generic minimum wall, die life, cooling time or heat-treatment recipe is asserted. The yield budget and handoff structure are original.

## Related reference

[Manufacturing processes](../index.md)