# EDM hole drilling

Electrical-discharge hole drilling: conductive materials, tubular electrodes and dielectric control, wear and breakthrough, geometry, surface integrity, and acceptance.

Reviewed: 2026-11-01

Tags: processes, shaping, edm, hole-drilling

A hypothetical **0.500 mm electrode** produces **0.560 mm entrance** and **0.540 mm exit** diameters over **10.000 mm axial length**. The ideal conical hole has **0.020 mm diametral taper**, **0.0573° half-angle** and **0.030 mm entrance radial excess** over the electrode. Inspect local bore geometry and account for electrode wear before attributing the excess to a discharge gap.

EDM drills small or difficult holes in conductive materials, including hardened metals. Account for electrode wear, dimensional error and thermal effects.

Specify full hole geometry and function, including access and breakthrough.

## Mechanism and neighboring EDM processes

Sodick identifies electrically conductive work materials as the scope of small-hole EDM, including hardened steels, cemented carbide, titanium, and superalloys. Conductivity, rather than ease of conventional cutting, is the essential starting requirement. The actual material, condition, thickness, and accuracy requirement still determine feasibility. [Sodick small-hole EDM](https://sodick.com/machines/small-hole-edm/)

| EDM route | Principal tool/path | Typical distinction |
| --- | --- | --- |
| Hole drilling | Slender electrode advanced along a hole path, often rotating and tubular | Deep/small holes and start holes; guide, flushing, wear and breakthrough control are central |
| Sinker EDM | Shaped electrode and programmed motion | Cavities and shaped details; some platforms also support precision hole operations |
| Wire EDM | Traveling wire following a programmed contour | Through-cut profiles; an internal contour may require a threading/start opening |

Do not equate the tube's outside diameter with the finished hole diameter. The discharge gap, electrode condition, motion, and process history affect the resulting geometry. Likewise, the machine's travel or maximum electrode length is not the guaranteed drilling depth in every material.

## Tubular electrodes, dielectric, and flushing

Sodick's **KIC Pipe(N)** is a two-hole copper electrode whose internal fluid passages and rotation support deep-hole machining without leaving a central core in the described application. This is an electrode-design feature; a simple hollow tube, multichannel tube, and solid microelectrode are not interchangeable solely because their outside diameters match. [Sodick KIC Pipe(N)](https://www.sodick.co.jp/en/product/supplies/pipe/kic-n.html)

Its **K3HS** machine page specifies deionized-water operation, copper/brass pipe-electrode machining conditions, an automatic electrode feeder, and through-hole detection. These details describe a particular machine configuration, not a universal requirement that every EDM hole drill use water. The manufacturer pages are undated here. [Sodick K3HS](https://www.sodick.co.jp/en/product/tool/drilling/item.php?id=k3hs)

Makino's *Selecting the Appropriate EDM Technology for Hole-Drilling Applications*, printed **©2014**, distinguishes oil- and water-based platforms. It discusses the tradeoffs among speed, spark gap, surface quality, precision, and finishing capability, and identifies filtration, deionization for water, and temperature control as process considerations. It also discusses worn-tip redressing and electrode management. Its historical capability examples are not current universal tolerance or aspect-ratio limits. [Makino white paper, pages 5–9](https://www.makino.com.sg/getmedia/6f72b909-980c-4779-941b-1d5d322a68bf/Makino_EDM_White_Paper_Final.pdf.aspx?ext=.pdf)

Specify the machine-approved fluid and maintenance controls, including temperature, filtration, and any conductivity/additive limits. Do not substitute untreated shop water or a different additive solely because another process uses it. An original **2007** study of **S50C steel**, using 20 mm-deep holes and an additive-containing aqueous fluid, found improved drilling/wear measures alongside reduced hole precision as additive quantity increased. It demonstrates a process tradeoff within its experiment, not a general fluid recipe. [Original ISIJ study](https://www.jstage.jst.go.jp/article/isijinternational/47/4/47_4_596/_article/-char/en)

## Access, wear, and breakthrough

Identify the entry surface, drilling angle, wall thickness along the electrode axis, internal cavities, and forbidden surfaces beyond breakthrough. A slender electrode requires appropriate guiding and clearance; its changing effective length and worn tip must be managed. A programmed Z travel alone is not a direct measurement of material removed because electrode consumption and part geometry also matter.

A bounded machine example is Makino's **EDBV3**, designed for blade/vane cooling features. Its page describes submerged deionized-water operation, a middle guide supporting long electrodes, electrode-length management, and a breakthrough circuit intended to prevent back-striking an internal rear wall. Its stated detection response belongs to that machine and configuration; it does not establish that another hole popper will protect a nearby wall. The page is undated and must be matched to the installed machine. [Makino EDBV3](https://www.makino.com/en-us/machine-technology/machines/edm-hole-drilling/edbv3)

For a hollow component, qualify the complete entry-to-breakthrough sequence and any subsequent shaped-hole operation. Establish how position, wall thickness variation, electrode wear, and stopping behavior are accommodated. Confirm the cavity remains free of unintended erosion and debris using suitable access or inspection methods.

## Taper, overcut, and an original example

The following is a **hypothetical geometry check**, not machine performance data. Assume a nominal **0.500 mm** electrode produces a hole with **0.560 mm entrance diameter**, **0.540 mm exit diameter**, and **10.000 mm axial length**. Model the hole as a straight, circular cone solely for this calculation.

| Quantity | Calculation | Result |
| --- | --- | --- |
| Diametral taper | 0.560 − 0.540 | 0.020 mm |
| Diameter change per axial length | 0.020 ÷ 10.000 | 0.002 mm/mm |
| Cone half-angle | atan[(0.560 − 0.540) / (2 × 10.000)] | 0.0573° |
| Included cone angle | Twice the half-angle | 0.1146° |
| Entrance radial excess over nominal electrode | (0.560 − 0.500) / 2 | 0.030 mm |

The last quantity is an apparent geometric excess, not a direct measurement of one instantaneous spark gap. Electrode wear and other process effects can contribute. The entrance and exit diameters also do not establish straightness, roundness, a local neck, or wall texture. A pin that passes through the minimum opening does not independently verify all those features.

For an angled hole, distinguish axial path length from component thickness normal to its faces. Define where diameters are evaluated and whether intentional diffuser geometry is excluded from a taper requirement.

## Recast, heat effects, and acceptance

Makino's white paper explicitly treats EDM drilling as thermal processing and identifies heat-affected material and recast as metallurgical-quality concerns. A favorable diameter or visually clean edge does not demonstrate acceptable surface integrity. [Makino white paper, page 4](https://www.makino.com.sg/getmedia/6f72b909-980c-4779-941b-1d5d322a68bf/Makino_EDM_White_Paper_Final.pdf.aspx?ext=.pdf)

An original recast-thinning study, first published online **17 December 2024** and appearing in **2025**, uses controlled discharge/finishing strategies for turbine film-cooling holes. It reports results for its tested method; those values are not generic as-drilled recast limits. Specify whether recast, cracks, affected material, or post-processing removal is restricted, and how the required state is verified. [Chu and colleagues, recast-thinning study](https://doi.org/10.1177/09544054241302679)

Separate geometric inspection from surface-integrity evaluation. Depending on the specification, evidence may include entrance/exit metrology, internal geometry measurement, sectioned representative specimens, metallography, or validated nondestructive methods. For fluid holes, a flow test establishes its test-condition response but cannot uniquely identify taper, obstruction, or microscopic cracking. Any finishing operation must preserve the required geometry and receive its own qualification.

A useful handoff contains four groups of information:

1. **Material and access:** alloy/condition, conductive path, entry surface, angle, axial depth, cavities, and forbidden back-wall regions.
2. **Hole definition:** diameters at stated locations, full geometry, datums, taper/straightness, edge requirements, and functional flow conditions.
3. **Qualified process:** installed machine, electrode/guide configuration, wear management, fluid controls, discharge strategy, breakthrough, and secondary finishing.
4. **Acceptance:** geometric and metallurgical limits, test methods/locations, representative specimens, sampling, cleanliness, and traceability.

## Related reference

[Manufacturing processes](../index.md)