# Solution heat treatment

Alloy-specific dissolution, cooling and subsequent-condition requirements, with separate solution, aging and acceptance controls.

Reviewed: 2026-11-01

Tags: processes, heat-treatment, solution-treatment

An example solution-treatment instruction allows **10 seconds from leaving the heated zone to full immersion**. The load arrives above the bath at **5 seconds**, starts lowering at **8 seconds** and reaches full immersion at **13 seconds**. The transfer exceeds the limit by **3 seconds**. Verify the defined events and load history. Use the qualified solution, quench and aging sequence for the alloy.

## What solution treatment establishes

Solution treatment dissolves specified constituents and cools the alloy to retain the required state. Natural or artificial aging is a separate step with its own acceptance requirements. [Bodycote solution and age](https://www.bodycote.com/what-we-do/precision-heat-treatment/solution-and-age-atmosphere-vacuum/)

Specify the alloy, product form, starting condition and intended final condition before selecting the cycle. “Solution treated” is neither one universal temperature nor a promise that the metal is dead soft. It is also not a direction to melt the workpiece or dissolve every constituent in an alloy.

## Keep the stages and output conditions separate

| Stage or condition | Question to resolve |
| --- | --- |
| Incoming material | Which phases, prior heat treatment, cold work and product form are present? |
| Heating and hold | What alloy-specific condition must be established throughout the relevant section? |
| Cooling | Which medium, transfer limits and cooling response preserve the required state? |
| Post-solution work and aging | Is forming, stretching, natural aging or artificial aging part of the required temper? |
| Final acceptance | Which properties and dimensions apply after the complete ordered route? |

A supplier's solution-treatment example should retain its specified cooling and subsequent treatment. Mixing the heating stage from one route with the aging stage from another can produce a condition for which neither source supplies evidence. Keep intermediate acceptance distinct from the delivered material condition.

## Aluminum: temper, cooling and elapsed time

Bodycote identifies heat-treatable wrought and cast aluminum families and describes cooling methods selected with alloy and section in mind. Its examples include liquid quench, spray and forced-air routes. These alternatives do not make all quench media interchangeable for every alloy or geometry. Select the qualified cooling route against the required properties and distortion limits. [Bodycote aluminum solution and age](https://www.bodycote.com/what-we-do/precision-heat-treatment/solution-and-age-atmosphere-vacuum/solution-and-age-aluminium-alloys/)

The same guidance distinguishes thermally produced tempers from conditions requiring additional thermomechanical work, such as stretching or compressing between solution treatment and aging. It also notes that natural aging after quenching changes hardness with elapsed time. Record that interval when forming or testing an as-quenched part; do not assume that reheating, storage or a new work order resets its metallurgical history. [Bodycote aluminum temper and sequence guidance](https://www.bodycote.com/what-we-do/precision-heat-treatment/solution-and-age-atmosphere-vacuum/solution-and-age-aluminium-alloys/)

Wrought products and castings also have different heat-treatment references. ASTM lists **B918/B918M-20a** for wrought aluminum and **B917/B917M-25** for aluminum-alloy castings. Choose the required product/process specification and contractual edition rather than applying a wrought-part procedure to a casting by analogy. Public catalog scopes are not complete furnace, quench or acceptance instructions. [ASTM B918/B918M-20a](https://store.astm.org/b0918_b0918m-20a.html), [ASTM B917/B917M-25](https://store.astm.org/b0917_b0917m-25.html)

## Stainless steel: the solution-treated structure matters

Outokumpu describes solution annealing after cold work and notes that the appropriate temperature and cooling depend on grade and purpose. It warns that incorrect temperature/time/cooling combinations can impair mechanical properties, toughness and corrosion resistance. Annealing in air can require removal of oxide scale to restore the surface. A specified final surface condition therefore belongs in the route, not only a furnace-temperature record. [Outokumpu solution annealing and surface restoration](https://www.outokumpu.com/en/expertise/stainless-basics/post-fabrication-treatment)

A different example is **Carpenter Custom 630 (17-4 PH)**. Its **v 4-24** datasheet describes solution-treated material as **Condition A** and specifically requires cooling below **90°F/32°C** to complete transformation to martensite before the later age-hardening step. Thus “solution treated” does not imply an austenitic room-temperature structure or the same condition as annealed austenitic stainless steel. [Carpenter Custom 630, printed page 7](https://www.carpentertechnology.com/hubfs/7407324/Material%20Saftey%20Data%20Sheets/Custom%20630%20%2817-4%20PH%29.pdf)

Carpenter also warns against using that Condition A without age hardening because of susceptibility to stress-corrosion cracking. This is a consequential limitation for the named alloy and producer guidance, not a universal prohibition on every solution-treated metal. State the required final aged condition and qualify the actual service environment. [Custom 630 solution-treatment limitation](https://www.carpentertechnology.com/hubfs/7407324/Material%20Saftey%20Data%20Sheets/Custom%20630%20%2817-4%20PH%29.pdf)

## Nickel alloy example: solution and age are a matched route

Special Metals' **INCONEL alloy 718 bulletin SMC-045, September 2007**, presents two common solution-anneal ranges, **1700–1850°F** and **1900–1950°F**, each followed by its corresponding rapid-cooling and precipitation-hardening sequence. Its discussion connects those complete routes to different strength, ductility and rupture behavior. The ranges are alternatives for that alloy and application, not a combined operating window or a modern universal acceptance specification. [Special Metals alloy 718, printed pages 2–3](https://www.specialmetals.com/documents/technical-bulletins/inconel/inconel-alloy-718.pdf)

Use the applicable producer recommendation and ordered specification for the actual product form and property objective. The bulletin's historic specification references and laboratory values do not automatically establish compliance with a later contractual issue. Do not detach an attractive property value from its complete treatment and specimen conditions.

## Load temperature, transfer and geometry

Define heating, hold, transfer, cooling and any post-treatment as one qualified route. Identify the reference events for each time limit, where load temperature is established, and how representative heavy or shielded regions are assessed. A furnace controller reaching setpoint is not itself evidence that the entire relevant section has achieved the required condition.

Review section changes, thin features, fixtures, assembly materials and permitted distortion with the processor. Preserve final size, form, surface condition and any machining allowance through the complete route. If a part is straightened, formed or stretched after cooling, record the operation and its relationship to the required material temper.

### Original bounded transfer-time example

Use the hypothetical **10-second maximum** from leaving the heated zone to full immersion:

| Event | Elapsed time from the specified start |
| --- | --- |
| Load leaves heated zone | 0 seconds |
| Load arrives above bath | 5 seconds |
| Lowering begins | 8 seconds |
| Full immersion | 13 seconds |

Timing only the five-second lowering operation uses the wrong start event. Qualify the transfer limit and resulting microstructure for the actual alloy and route.

## Acceptance and manufacturing handoff

Define the tested state and sampling before processing. Depending on the product specification, acceptance may involve mechanical properties, hardness, conductivity, structure, surface condition and dimensions. These measurements answer different questions; a hardness value alone cannot prove complete dissolution, required corrosion performance or the correct later-aged condition.

Provide material/heat identity, starting temper, drawing revision, product form and section sizes, governing specification/edition, required solution and final conditions, approved sequence and any prohibited property changes. Agree lot/load traceability, test locations, cooling and elapsed-time records, sampling, dimensional inspection and deviation disposition. A certificate should identify the treatment actually performed and the output requirements it satisfies.

Source versions: Carpenter prints **©2024, v 4-24** on its final page; Special Metals prints **SMC-045, ©2007 (Sept 07)**. The ASTM editions above are those listed by the publisher. No verified technical issue date is assigned to the supplier web descriptions. The transfer-time example is original.

## Related reference

[Grades, tempers and conditions](../../materials/grades-tempers-and-conditions.md)