# Abrasive blasting

Specifying a blast-cleaning process and separately accepting visual cleanliness, profile, contamination and coating readiness.

Reviewed: 2026-11-01

Tags: processes, finishing, abrasive-blasting, surface-preparation

[Compare surface-finishing options](../surface-finishing.md) before specifying the complete route.

A profile of **0.0025 in converts to 63.5 µm**. A profile of **0.0035 in converts to 88.9 µm**, or **13.9 µm over** the worked example's **50–75 µm** range. Compare readings using the agreed profile method, sampling locations and uncertainty rule. Verify cleanliness separately.


## Process and scope

This guide covers steel preparation before protective coating. Specify cleanliness, profile and the abrasive procedure for that coating system.

**ISO 8504-2:2019**, edition 3, October 2019, covers abrasive blast-cleaning methods for steel before coating, including equipment, procedures, effectiveness and application. Its public record remains published and marked for revision. The scope notes that cold-rolled steel must be sufficiently thick to withstand deformation from abrasive impact; suitability is not established merely because a part is made of steel. [ISO blast-cleaning method scope](https://www.iso.org/standard/72939.html)

Specify the substrate, initial condition, process variant and required result. Do not use “sandblast” as a complete material or acceptance specification. A process developed for a thick structural member should not automatically be transferred to a thin precision component, sealing surface or finished thread.

## Four different acceptance questions

AMPP's surface-preparation committee distinguishes abrasive media, cleanliness levels for dry/wet cleaning, non-visible contaminants and surface-profile depth/density as separate subjects. These need corresponding requirements and evidence. [AMPP SC 05 surface preparation](https://www.ampp.org/standards/sc-05-surface-preparation)

| Question | Definition to agree before work |
| --- | --- |
| Visual cleanliness | Governing standard, initial condition and required preparation grade |
| Surface profile | Required characteristic/range and compatible measurement method |
| Contamination | Relevant salts, dust, oil or other contaminants and test/acceptance requirements |
| Coating readiness | Coating-system instructions, environmental limits and permitted exposure before coating |

A photograph of clean-looking steel does not supply a measured profile or contamination result. Likewise, an acceptable profile reading does not establish removal of every contaminant. Keep these results separate in the inspection record.

## Visual cleanliness versus profile

**ISO 8501-1:2007**, edition 2, May 2007, confirmed in 2017, defines steel rust/preparation grades through written descriptions and representative photographs. Its scope concerns steel preparation for painting; the written and photographic definitions belong together. Identify the applicable initial condition and method rather than comparing a surface to an unrelated photograph. [ISO visual-assessment scope](https://www.iso.org/standard/43426.html)

Elcometer explicitly distinguishes pictorial cleanliness standards from profile assessment. Its preparation guidance also treats non-visible contamination testing separately and directs acceptance to the job/coating specification. Do not assume that an ISO preparation grade and an SSPC/AMPP designation are interchangeable without the contract defining the requirement. [Elcometer inspection after preparation](https://www.elcometer.com/en/inspection-after-surface-preparation)

Profile is the resulting surface texture relevant to coating application. Agree the specified characteristic and measurement method; a comparator, depth gauge, replica-tape method and stylus instrument do not automatically report interchangeable quantities. Avoid treating a generic machining roughness value as the complete blast-profile requirement.

**ISO 8503-5:2017**, edition 2, March 2017, confirmed in 2022, describes field measurement using replica tape and a suitable gauge. Its scope limits use to the profile-height range for the selected tape grade. That range is a measurement-method constraint, not a recommended target for every coating. [ISO replica-tape method](https://www.iso.org/standard/60139.html)

## Inputs, media and process qualification

Document the chosen abrasive, delivery condition and process variant, together with equipment settings and coverage needed to reproduce the qualified result. Establish access, masking, protected dimensions and acceptable material removal before production. Use representative trials where impact, edge erosion or distortion could affect function. These are proposed process-development questions rather than a universal nozzle-pressure, stand-off or dwell recipe.

Recycled media and water can introduce contamination. Elcometer's process guidance discusses monitoring their cleanliness, including soluble salts, and checking environmental conditions before blasting when coating will follow. Condensation can lead to oxidation of the prepared surface. [Elcometer inspection during blasting](https://www.elcometer.com/en/inspection-during-the-blasting-process)

Preserve media control and cleaning instructions with the job. A fresh-looking surface is not a reason to omit specified contamination tests. If reblasting changes the surface after inspection, repeat the relevant acceptance checks for the final condition rather than relying on the earlier result.

## Original unit-conversion example

Use the illustrative **50–75 µm** contract range and the exact conversion of 25.4 mm per inch:

`0.0025 in × 25,400 µm/in = 63.5 µm`

`0.0035 in × 25,400 µm/in = 88.9 µm`.

Compare these converted values using the specified method and uncertainty. Sample difficult-to-reach areas, transitions and locations with different exposure to the abrasive stream.

Do not substitute an average for the contract's stated acceptance rule. Preserve individual locations/results where required, especially around difficult access, transitions and regions with different exposure to the abrasive stream.

## Worker and environmental controls

OSHA's abrasive-blasting fact sheet identifies dust, noise and hazardous substances in both the abrasive and the material/coating being removed. It describes evaluating hazards and using appropriate substitution, engineering controls, work practices and protective equipment. A medium described as less toxic does not remove the hazards of the substrate or old coating. [OSHA abrasive-blasting fact sheet](https://www.osha.gov/sites/default/files/publications/OSHA3697.pdf)

Plan containment, extraction, waste handling and worker protection for the actual material and site. The technical surface requirement is only one input to that plan. This article supplies no exposure-limit calculation, respiratory-protection selection or site-specific compliance procedure.

## Handoff and release

Retain the part/job revision, substrate and initial condition, selected process/media, protected areas, visual standard/grade, profile requirement/method/results, contamination results, environmental records and final inspection time. Identify the coating system and its preparation requirements, and resolve delay, recontamination or changed conditions before coating.

Inspect the finished preparation against the agreed criteria and preserve exceptions. If an inaccessible region or protected feature needs a different method, define it explicitly rather than silently calling the whole component uniformly blasted. These are practical handoff fields rather than a normative inspection template.

## Source scope

ISO dates above distinguish publication, confirmation and revision status. The public scopes do not reproduce the normative procedures or grade photographs. AMPP and Elcometer live guidance have no verified technical revision date here; no issue date is inferred from a website copyright. The unit arithmetic and proposed process/handoff questions are original guidance.