# Type 430 stainless steel

Unstabilized ferritic UNS S43000: product-specific properties, surface and forming choices, and weld/service limitations.

Reviewed: 2026-11-01

Tags: materials, stainless-steel, ferritic

## Identity and selection

ATI's ASTM A240 **Type 430 sheet and strip** listing gives **22% minimum elongation**, with a thickness note of **20% at 1.27 mm and thinner**. It also lists **450 MPa minimum tensile**, **205 MPa minimum yield**, and **89 HRB maximum**. Use the ordered edition and its test provisions for acceptance. [ATI sheet and strip summary](https://www.atimaterials.com/Products/Pages/ati-430.aspx)

Type 430 is **UNS S43000**, a ferritic stainless steel. ATI's sheet/strip product page lists **16–18% chromium** and **carbon ≤0.12%**, with other controlled elements. Outokumpu identifies its Moda 430/4016 as an **unstabilized**, non-hardenable ferritic product associated with **EN 1.4016**, used particularly in mildly corrosive indoor environments. [ATI product page](https://www.atimaterials.com/Products/Pages/ati-430.aspx), [Outokumpu Moda range](https://www.outokumpu.com/en/products/product-ranges/moda)

Keep ordinary 430 separate from stabilized 430Ti, free-machining variants and austenitic 304. A shared number fragment does not establish equivalent fabrication behavior. Specify the complete grade, governing standard and edition, form, dimensions, supplied condition, finish and inspection documents.

Select against the component's actual exposure and manufacturing route. For trim or a formed appliance panel, appearance and drawability may govern alongside corrosion; for a load-bearing part, the applicable design rules and delivered material evidence must also be established.

## Mechanical values: retain the product and standard

ATI's technical bulletin separately reports **typical room-temperature** properties of cold-rolled, annealed sheet/strip: for **0.02–0.06 inch** thickness, 0.2% yield strength **44–54 ksi**, tensile strength **70–79 ksi**, and elongation in 2 inches **21–34%**. These summarized longitudinal/transverse results are characterization data, not substitute acceptance minima. [ATI bulletin, mechanical properties and footnotes](https://www.atimaterials.com/Products/Documents/datasheets/stainless-specialty-steel/ferritic/ati_430_tds_en.pdf)

Do not combine a typical tensile result, a minimum yield requirement and an elongation measured on a different gauge length into an invented material condition. Preserve test direction, temperature, thickness, finish, cold reduction and certificate identity with calculation inputs. A visible finish may include processing that changes properties.

## Corrosion and surface acceptance

Outokumpu reports lower resistance to localized chloride corrosion for Moda 430/4016 than for its 304/4301 or 304L/4307 products. Its strong ferritic resistance to chloride-induced stress corrosion cracking does not remove pitting or crevice-corrosion concerns. [Moda bulletin, corrosion discussion](https://www.outokumpu.com/-/media/files/products/moda/outokumpu-moda-range-datasheet.pdf)

Record chlorides, temperature, wet/dry cycles, deposits, crevices and cleaning chemicals. Include hidden joints and shutdown conditions. Define an acceptable cosmetic condition separately from a structural corrosion allowance; an application name such as “kitchen equipment” does not qualify every cleaning or food-contact duty.

For an appearance-critical part, approve a finished sample after the intended forming, joining and cleaning sequence. Keep grain direction, scratch acceptance and inspection lighting in the purchasing record. Surface treatment does not change the bulk grade into a more highly alloyed stainless.

## Forming and welding

ATI describes **earing** in deep drawing and **roping**, surface striations parallel to the rolling direction, during some forming operations. Its relatively low work-hardening rate also limits stretch forming compared with austenitic grades. [ATI bulletin, deep drawing and roping](https://www.atimaterials.com/Products/Documents/datasheets/stainless-specialty-steel/ferritic/ati_430_tds_en.pdf)

Qualify blank orientation, tooling, lubrication, radii and cosmetic acceptance on representative stock. Tensile elongation alone cannot predict the outcome of a complex draw. Inspect the final surface and dimensions after operations that can alter them.

Outokumpu explicitly says Moda 430/4016 is **not intended for the as-welded condition** and gives **750–800°C postweld heat treatment** for adequate weld-region ductility and corrosion resistance. This is producer guidance requiring a qualified component process. [Moda bulletin, weldability](https://www.outokumpu.com/-/media/files/products/moda/outokumpu-moda-range-datasheet.pdf)

Before selecting it for a welded assembly, resolve filler, joint geometry, restraint, thermal sequence, final properties and cleaning. Establish whether the assembly can tolerate the required treatment and resulting distortion. If it cannot, reconsider the material or joint rather than assuming the starting sheet properties apply across the weld.

## Thermal exposure and a bounded calculation

ATI's oxidation guidance gives **870°C intermittent** and **790–815°C continuous** exposure, while emphasizing atmosphere, cycling and design dependence. Those values do not establish permissible stress, creep life or retained toughness. Its bulletin also warns of reduced impact properties after several days at **425–540°C**. [ATI bulletin, oxidation and impact sections](https://www.atimaterials.com/Products/Documents/datasheets/stainless-specialty-steel/ferritic/ati_430_tds_en.pdf)

Keep oxidation, mechanical loading and thermal aging as separate selection questions. Record metal temperature, time and cycles, including fabrication and upset exposure; one maximum-temperature field cannot represent all of them.

**Original free-expansion example:** Moda's reference coefficient is **10.0 × 10⁻⁶/K over 20–100°C**. A uniformly heated, freely expanding 1,000 mm strip over that interval gives `ΔL = 1000 × 10.0 × 10⁻⁶ × 80 = 0.80 mm`. Restraint, thermal gradients, joints and buckling are excluded; this is not a stress or clearance qualification. [Moda bulletin, table 6](https://www.outokumpu.com/-/media/files/products/moda/outokumpu-moda-range-datasheet.pdf)

## Procurement record and source versions

Retain producer, heat/lot, standard edition, form, thickness, condition, finish, certificate, processing route and required final inspections. Record approved substitutions against the complete requirement, including weld and surface acceptance.

ATI's inspected bulletin prints **Version 1, 13 July 2012**. The inspected Moda bulletin prints **October 2022**; its URL modification date is not its technical edition. No technical revision date was verified for the live product pages. These references do not establish the current contractual standard edition.

See [grades, tempers and conditions](../grades-tempers-and-conditions.md).