# G10 glass-epoxy laminate

Selecting and specifying woven-glass epoxy laminate by grade, stock form, test direction and service conditions.

Reviewed: 2026-11-01

Tags: materials, composites, electrical-insulation

Norplex’s **NP500A G-10 sheet** has typical **ASTM D790 Condition A** flexural strength of **455.1 MPa lengthwise** and **413.7 MPa crosswise**. Using the lengthwise value across the sheet overstates the reported result by **41.4 MPa (10.0%)**. Qualify the actual laminate direction and loading before setting a working stress. [Norplex NP500A technical data bulletin](https://www.norplex-micarta.com/wp-content/uploads/2017/07/TDB_NP500A.pdf)

G-10 is a grade of cured glass-cloth/epoxy laminate used for electrical insulation and mechanical support. It is a starting point for material selection, rather than one resin recipe or a complete structural specification. Norplex explains that manufacturers can vary glass weight, chemistry and processing while meeting the grade requirements. Its NP500A sheet and RT500 tube, for example, use different chemistries despite both meeting G-10 requirements. [Norplex: What is G-10?](https://www.norplex-micarta.com/structural-materials/what-is-g-10/)

## Identify the actual material

Specify the manufacturer, product designation, governing material specification and revision, stock form, thickness and required certification. Include reinforcement orientation when it affects the component. A purchase description of “green G10” leaves important decisions unresolved: color does not establish resin chemistry, flame performance or acceptance values.

Norplex NP500A is woven glass with non-brominated epoxy, sold for structural support and insulation; the manufacturer explicitly calls it non-flame-retardant. Conversely, Accurate Plastics markets **Acculam Epoxyglas G10/FR4**, whose data sheet identifies flame-retardant epoxy and qualification to **NEMA FR4 and MIL-I-24768/27**. A slash in a commercial name does not establish that every G-10 and FR-4 requirement is interchangeable. Resolve the required grade with the supplier before substitution. [NP500A product description](https://www.norplex-micarta.com/grades/NP500A/), [Acculam data sheet, Rev 08.01.24](https://acculam.com/Portals/0/Acculam-Epoxyglas-G10-FR4-Data-Sheet.pdf)

Treat sheet, rolled tube and rod as separate products. A ring machined from a sheet and one cut from tube do not automatically have equivalent reinforcement directions or qualification data. Likewise, ordinary G-10 should not inherit the performance of a specialized cryogenic grade simply because its name includes G-10. Norplex specifically distinguishes G-10 from G-10CR. [Norplex grade explanation](https://www.norplex-micarta.com/structural-materials/what-is-g-10/)

## Read properties with their directions and conditions

Retain the supplier’s lengthwise, crosswise, flatwise and edgewise labels relative to the part and load.

For a bounded comparison, Norplex's **NP500A bulletin dated July 14, 2022** lists these **typical**, Condition A results:

| Property and method | Lengthwise | Crosswise |
| --- | --- | --- |
| Flexural strength, ASTM D790 | 455.1 MPa | 413.7 MPa |
| Tensile strength, ASTM D638 | 296.5 MPa | 268.9 MPa |

The bulletin explicitly says typical values are not specification values and asks specification writers to obtain acceptance values. These results are neither working stresses nor evidence for a different thickness, orientation or environmental condition. [NP500A technical data bulletin](https://www.norplex-micarta.com/wp-content/uploads/2017/07/TDB_NP500A.pdf)

Hole bearing, fastener pull-through, laminate separation, sustained loading and actual service temperature still require design evidence.

## Electrical and thermal limits

Separate breakdown voltage in kV from electric strength in kV/mm. MICAM's **EG-10 sheet EG10.2021.03** reports flatwise dielectric strength **14 MV/m at 1.6 mm**, and edgewise dielectric strength **60 kV at 3 mm**, both under IEC 243-1. The different units and directions matter: these entries cannot be compared as two thickness-normalized strengths. The sheet also reports permittivity **4.3 at 1 MHz** and calls its results laboratory typical/average values, not specifications or guarantees. [MICAM EG-10 data sheet](https://www.micam.com/technical-data-sheet/MICAM.EG10.pdf)

An electrical component therefore needs an application assessment covering electrode geometry, clearances, creepage, contamination, moisture, frequency and temperature. Multiplying a coupon strength by a finished spacer's thickness is not an allowable-voltage calculation. Document the actual insulation function and required verification rather than assigning a voltage rating from the material name.

MICAM reports an IEC 216 thermal index of **130°C**, while Norplex cautions that the maximum operating temperature depends on the application. Thermal index, glass-transition temperature and an allowable loaded service temperature answer different questions. Norplex also notes that its discussion of the G-10 electrical grade does not establish a minimum glass-transition temperature. Obtain product-specific hot/wet and elevated-temperature data where stiffness or dimensional stability controls the design. [MICAM EG-10](https://www.micam.com/technical-data-sheet/MICAM.EG10.pdf), [NP500A bulletin](https://www.norplex-micarta.com/wp-content/uploads/2017/07/TDB_NP500A.pdf), [Norplex grade explanation](https://www.norplex-micarta.com/structural-materials/what-is-g-10/)

## Stock allowance and fabrication

Nominal sheet thickness is not finished-part thickness. Norplex's **April 6, 2020** tolerance guide gives NP500-series glass sheet at nominal **0.125 in** a listed tolerance of **±0.012 in**, with an area-based qualification: at least 90% must meet the table, and no point may exceed 125% of its tolerance. Specify machined thickness, flatness and inspection requirements separately when the component requires closer control. [Norplex sheet tolerances](https://www.norplex-micarta.com/wp-content/uploads/2017/08/Tolerances_Sheets.pdf)

Norplex's fabrication guide recommends diamond or tungsten-carbide tooling for glass-based grades, carbide drills, and climb milling to reduce delamination. It advises predrilling waterjet pierce locations. Its adhesive guidance calls for sanding and cleaning followed by a two-part epoxy appropriate to the environment. These are starting recommendations, not a qualified recipe for every machine, adhesive or laminate. [Norplex fabrication guide](https://www.norplex-micarta.com/wp-content/uploads/2017/07/Fab_Guide.pdf)

For a new part, agree on acceptable edge breakout, exposed fibers, cracking, delamination and surface condition with the fabricator. Trial the actual stock and toolpath, inspect holes and cut edges, and verify dimensions after processing. Bonded assemblies need their own preparation, adhesive, cure and environmental qualification; a laminate's internal “bond strength” result is not an adhesive-joint rating.

## Handling and specification checklist

Norplex SDS **ILN0228A**, which explicitly includes NP500A, identifies no hazards for the product as shipped but identifies respiratory, skin and eye irritation and combustible-dust hazards after processing. It calls for local exhaust, suitable skin/eye protection and an approved dust respirator when exposure exceeds applicable guidelines. Thermal decomposition introduces additional hazards. Plan dust collection and housekeeping before machining; an intact-sheet classification does not describe airborne machining debris. The SDS's **last revision is June 12, 2018**; **June 10, 2024 is its print date**. [Norplex SDS](https://www.norplex-micarta.com/wp-content/uploads/2017/07/SDS_ILN0228A.pdf)

A useful release record includes the exact stock grade/form; relevant specification and acceptance certificate; material directions; dimensional and edge-quality requirements; electrical, mechanical and thermal service conditions; and the evidence supporting the finished component. Record chemical exposure by substance, concentration, temperature and duration rather than relying on an unqualified “chemical resistant” description.

## Source scope

The product pages were checked for this review. PDF dates above are printed document identifiers, not website upload dates. The two-page fabrication guide has no visible revision date. Supplier examples describe those products only; required fire, electrical or structural approvals must be established for the intended assembly.

## Related reference

[Material selection through production](../grades-tempers-and-conditions.md)