# 5083 aluminum

5083 alloy, product-form and temper distinctions, marine corrosion-test scope, and forming and welded-service limitations.

Reviewed: 2026-11-01

Tags: materials, aluminum, marine-materials

## Alloy identity and product scope

Hulamin lists **125 MPa minimum proof stress, 275 MPa minimum tensile strength and 15% minimum elongation** for 5083-H111. Its H116/H321 entry lists **215 MPa, 305 MPa and 10%** respectively. Corrosion testing and after-weld properties require separate evidence. [Hulamin marine and transport plate](https://www.hulamin.com/sites/default/files/downloads/5083%20Data%20Sheet.pdf)

5083 is a wrought aluminum–magnesium–manganese alloy. The Aluminum Association's **Teal Sheets, revised December 2025**, specify magnesium at 4.0–4.9%, manganese at 0.40–1.0% and chromium at 0.05–0.25% by mass. Registered composition identifies the alloy; it does not specify a temper, manufacturing route or marine approval. [Aluminum Association, Teal Sheets, 5083 entry](https://www.aluminum.org/sites/default/files/2026-01/Teal%20Sheets%20December%202025.pdf)

Hydro describes 5083 as non-heat-treatable, with strength derived from composition and strain hardening rather than precipitation aging. Sheet and plate are common, while selected extrusion applications also exist. Do not transfer plate values to an extrusion or treat a product list as evidence that every form is available from every supplier. [Hydro, 5083 alloy](https://www.hydro.com/us/global/aluminum/products/extruded-profiles/alloys-for-aluminum-extrusions/5083-alloy/)

Specify **alloy + temper + product form + size + applicable standard/edition + inspection requirements**. Include required corrosion testing, surface condition and material certification. A description such as “5083 marine grade” omits essential acceptance conditions.

## Temper and thickness change the property claim

Aalco describes O as soft and H111 as having some shaping-induced work hardening, less than H11. Its O/H111 page reports 125 MPa minimum proof stress and 275–350 MPa tensile strength for 0.2–6.3 mm sheet, versus 115 MPa minimum and 270–345 MPa for 6.3–80 mm plate. It labels the information indicative and references BS EN 485-2:2008 for these summaries. Confirm the ordered standard and exact dimensional band before acceptance. [Aalco, 5083 O/H111 sheet and plate](https://www.aalco.co.uk/datasheets/Aluminium-Alloy_5083-0~H111_149.ashx)

Hulamin's undated **5083 Rolled Products Data Sheet** publishes these separate temper entries:

| Temper grouping in supplier sheet | Proof stress, minimum | Tensile strength | Minimum elongation |
| --- | --- | --- | --- |
| H111 | 125 MPa | 275 MPa minimum | 15% |
| H32 | 215 MPa | 305–380 MPa | 8% |
| H116 / H321 | 215 MPa | 305 MPa minimum | 10% |
| H34 | 250 MPa | 350 MPa minimum | 6% |

The table lacks complete thickness/direction/specimen scope. Confirm applicability before treating these supplier entries as acceptance limits. [Hulamin 5083 rolled-product datasheet](https://www.hulamin.com/sites/default/files/downloads/5083%20Data%20Sheet.pdf)

**Bounded comparison:** Hulamin's H111 and H116/H321 rows differ by 90 MPa in published minimum proof stress (215 − 125). That arithmetic illustrates temper dependence; it does not establish a finished structure's allowable load or authorize substitution. A stronger temper may also require a different forming route and corrosion-test evidence.

Keep the property definition, direction, specimen location, gauge length, thickness range and value status with each number. A minimum, a typical value and a design allowable serve different purposes. Do not combine strength from one product table with elongation from another to invent a preferred condition.

## H116/H321 and marine corrosion evidence

The Aluminum Association's **May 2009** comparative-characteristics footnote explains that H116/H321 products are used where intergranular and exfoliation corrosion resistance must be demonstrated. It explicitly warns against replacing these products with H32 based on similar tensile properties, because the corrosion-testing requirements differ. This historical guidance explains the distinction; the current contract and applicable standard govern actual acceptance. [Aluminum Association, Table 3.3, footnote 8](https://www.aluminum.org/sites/default/files/2022-12/Table_3.3.pdf)

ASTM's B928/B928M publication is specifically titled **High Magnesium Aluminum-Alloy Products for Marine Service and Similar Environments**. Identify the required edition and covered product rather than assuming a general sheet specification or a “marine” stock description provides the same requirements. [ASTM B928/B928M-15(2023), publication record](https://store.astm.org/b0928_b0928m-15r23.html)

For procurement, distinguish the material designation, the specified corrosion tests and their actual results, and any classification-society approval. One does not establish the others. Verify that certificates identify the supplied lot, relevant product dimensions and required tests; keep those records linked to cut parts. Do not invent corrosion-test thresholds from a generic datasheet.

## Forming and machining

Hulamin gives bend radii of 1.5t for H111 and 2.5t for H116/H321, limited to thickness t ≤6 mm. Confirm tooling/orientation applicability. [Hulamin 5083 forming table](https://www.hulamin.com/sites/default/files/downloads/5083%20Data%20Sheet.pdf)

Qualify bend angle, inside radius, grain direction, edge preparation, tooling and springback on the intended material. Inspect cracking, thinning and surface marks against drawing requirements. A successful coupon in H111 does not qualify the same bend in a stronger temper. If heating is proposed to aid forming, assess the final strength and corrosion condition rather than assuming the original certificate still describes the finished region.

For machined plate components, plan workholding, stock removal and inspection around actual geometry. Catalog material strength does not promise flatness after pocketing or dimensional stability after welding. Retain surface-treatment allowances and inspect critical dimensions after the operations that can change them.

## Joining and heat-affected zones

Hydro explains that fusion welding softens cold-worked non-heat-treatable aluminum around the weld. A statement that 5083 welds well therefore does not justify assigning unwelded H116 strength to an entire welded assembly. Distinguish weld metal, heat-affected zone and unaffected parent in design and inspection. [Hydro, aluminum welding rods and HAZ behavior](https://www.hydro.com/us/us/aluminum/products/extruded-profiles/north-america-resources/extruded-aluminum-products/aluminum-rod/aluminum-welding-rods/)

Hulamin lists 5183 and 5356 TIG/MIG fillers. Confirm selection for both alloys, strength, corrosion exposure and service temperature through a qualified procedure. [Hulamin 5083 joining guidance](https://www.hulamin.com/sites/default/files/downloads/5083%20Data%20Sheet.pdf)

Define joint preparation, cleanliness, heat input, distortion control, inspection and leak testing where required. Account for attachments and repair welds too. A parent-material certificate cannot establish final weld soundness, fatigue life or the corrosion performance of a thermally altered assembly.

## Service exposure and temperature

Hydro lists marine, offshore, transport-tank and cryogenic applications. Those are application families, not approval for every cargo, pressure, loading cycle or minimum design temperature. Select product specifications and design properties for the actual service. [Hydro 5083 application guidance](https://www.hydro.com/us/global/aluminum/products/extruded-profiles/alloys-for-aluminum-extrusions/5083-alloy/)

Aalco does not recommend its 5083 O/H111 offering for temperatures above 65°C. Preserve this supplier warning and obtain application-specific advice for elevated-temperature exposure. Do not interpret it as a guaranteed safe continuous-service rating at 65°C, a permission for arbitrary excursions, or a universal sensitization boundary independent of exposure duration and condition. [Aalco 5083 service guidance](https://www.aalco.co.uk/datasheets/Aluminium-Alloy_5083-0~H111_149.ashx)

Assess exposure history, wet crevices, dissimilar-metal contact, coatings and cleaning agents. Marine corrosion resistance does not imply chemical immunity, zero maintenance or an assigned service life. Define the protection and inspection plan for the fabricated assembly rather than relying on the word “marine.”

## Traceable selection and release

Keep batch identity, supplied temper and process history linked through cutting, forming and joining. Record whether a quoted property is a supplier summary, specification limit, tested batch result or design value. Resolve missing thickness scope, temper substitutions and corrosion-test requirements before release, and retain the actual source edition with the capability record.

## Related reference

[Grades, tempers and conditions](../grades-tempers-and-conditions.md)