# Cross-cut adhesion testing

Coating separation ratings, method and cutter selection, tape controls, and limits of cross-cut test interpretation.

Reviewed: 2026-11-01

Tags: inspection, coatings, adhesion, destructive-testing

## What the test establishes

Cross-cut testing classifies local coating separation after a lattice is cut through to the substrate and loose material is removed. Record the procedure with the result.

**ISO 2409:2020**, published August 2020, describes an empirical resistance-to-separation test and explicitly states that it is **not a measurement of adhesion**. It permits pass/fail use or a six-step classification where appropriate. The public scope excludes total coating thickness above **250 μm** and textured coatings and distinguishes procedures for hard and soft substrates. For multilayer systems, separation can occur between coats. [ISO: ISO 2409 scope](https://www.iso.org/standard/76041.html)

A cross-cut classification does not provide a tensile bond strength in MPa. ISO's scope points to ISO 4624 where adhesion measurement is required. It also does not establish weathering life, corrosion protection, or performance after an exposure that was never tested.

## Select the standard before the tool

**ASTM D3359-23** covers pressure-sensitive tape tests on relatively ductile coatings applied to metallic substrates. Its Method A uses an X-cut; Method B uses a lattice. Method B is primarily intended below **125 μm** total thickness; thicker films require the specified wider-cut exception and explicit purchaser/seller agreement. ASTM identifies ISO 2409 as similar but **not technically equivalent**. [ASTM: D3359-23 scope](https://store.astm.org/d3359-23.html)

| Inspection input | Decision it controls |
| --- | --- |
| Standard, method, and edition | Applicable procedure, classification, and reporting requirements |
| Total dry-film thickness | Cutter spacing and method applicability |
| Substrate type and hardness | Support, cutting behavior, and applicable spacing |
| Coating system and cure condition | What material condition the result represents |
| Geometry and texture | Whether a valid lattice can be produced and assessed |
| Exposure history | Whether the test represents initial, immersed, aged, or service-exposed condition |

Establish the required classification or acceptance threshold separately from the method. A test-method designation alone does not supply the product's acceptance requirement. Confirm the drawing, coating specification, or agreed inspection plan before cutting a finished part.

## Cutter spacing and a bounded equipment example

DeFelsko's **PosiTest CH literature, copyright 2023, document DTv.LW-W2307**, lists these ISO 2409 kit arrangements:

| Listed coating thickness | Blade spacing and teeth | Kit |
| --- | --- | --- |
| 0–60 μm, hard substrate | 1 mm, six teeth | CHKITISO6X1 |
| 61–120 μm | 2 mm, six teeth | CHKITISO6X2 |
| 121–250 μm | 3 mm, six teeth | CHKITISO6X3 |

Its soft-substrate footnote specifies **2 mm/six teeth for 0–120 μm**. The same sheet separately lists ASTM kits with **1 mm/eleven teeth for 0–50 μm** and **2 mm/six teeth for 51–125 μm**. These are documented product-selection entries, not permission to mix procedures or extend thickness limits. [DeFelsko: PosiTest CH kit and blade tables](https://dl.defelsko.com/pdf/literature/PosiTestCH.pdf)

**Illustrative selection:** an assumed 40 μm coating on wood would lead to the soft-substrate ISO selection, not the hard-substrate 1 mm selection. A 90 μm coating on metal falls in different method-specific tables even when both identify a 2 mm blade. Matching blade spacing alone does not make the tests equivalent.

## Preparation and cut quality

Determine dry-film thickness before selecting the cutter. Define the test locations and specimen condition, including cure, conditioning, and any prior exposure. Support the specimen so the cutter can produce controlled cuts without panel movement.

DeFelsko's **instruction manual ICH.v.1.0-0723, copyright 2023**, directs inspection of cutting edges for wear or damage and replacement or rotation to an unused edge as appropriate. It requires cuts to reach the substrate and identifies inadequate penetration as invalid. Its ISO laboratory preparation includes **23 ±2 °C**, **50 ±5% relative humidity**, and at least **16 hours** of panel conditioning; do not silently apply laboratory conditioning as a description of an uncontrolled field test. [DeFelsko: manual, preparation and ISO sections](https://dl.defelsko.com/pdf/manuals/PosiTestCH-InstructionManual.pdf)

Elcometer emphasizes even load across the blade and choosing cutter spacing and blade count for the standard and film thickness. A multi-blade tool still needs correct handling: excessive tearing, incomplete cuts, or uneven contact can obscure coating behavior. Inspect the lattice before interpreting material removal. [Elcometer: cross-hatch method](https://www.elcometer.com/en/cross-hatch-method)

Do not repeatedly recut the same damaged area to obtain a desired classification. Preserve photographs of the lattice and any preparation problem, and repeat invalid tests at suitable fresh locations under the governing procedure.

## Tape and removal procedure

Tape is a test consumable, not an interchangeable household supply. Identify its product, lot where available, condition, and applicable specification. Control application, dwell, removal direction and speed, and assessment timing according to the chosen method.

The DeFelsko manual's ISO summary allows an agreed loose-paint removal method, including tape or brushing. Its tape example uses a **60°** pull, while its ASTM summary specifies pulling tape back over itself near **180°**. These angles belong to different described procedures. Do not combine a cutter from one method with another method's tape handling and then report an unqualified standard classification. [DeFelsko: method-specific removal instructions](https://dl.defelsko.com/pdf/manuals/PosiTestCH-InstructionManual.pdf)

ASTM D3359's public significance statement explains that tape behavior depends on the coating and that removal angle and rate affect the result. It also cautions that the method does not distinguish fine differences among higher adhesion levels. [ASTM: significance and operator effects](https://store.astm.org/d3359-23.html)

## Classification and failure location

Use the applicable descriptions and reference images, not percentage estimates alone. The numbering direction differs: HMG Paints' **KNB0019, dated 19 May 2006**, illustrates smooth cuts with no detached squares as **ISO class 0** and **ASTM class 5B**. That historical comparison helps avoid reversing the rating, but does not replace the current method's classification rules or establish technical equivalence. [HMG Paints: cross-hatch classification guide](https://www.hmgpaint.com/knowledge/knowledge-base/70/cross-hatch-test-classification)

Describe the interface where separation appears to have occurred. Removal between two coats is different from separation at the substrate; torn substrate or cohesive coating failure warrants its own observation. Do not infer substrate adhesion when the observed failure never reached that interface.

DeFelsko's ASTM Method B guidance includes reporting the substrate, coating and cure information, number and spread of results, tape identification or measured adhesion information, estimated failure interface, and immersion conditions where applicable. Preserve those conditions when comparing suppliers or repeated tests. [DeFelsko: ASTM Method B reporting guidance](https://www.defelsko.com/resources/how-to-perform-a-cross-hatch-adhesion-test-in-accordance-with-astm-d3359-method-b)

## Interpretation and records

Record each location and classification with images, cutter identity and condition, measured film thickness, method edition, removal procedure, tape details, coating age/cure, environment, exposure, and acceptance criterion. Report deviations explicitly. A high classification under one condition does not establish performance on every production surface or after aging.

Use cross-cut testing as the defined local empirical assessment. If the engineering question requires quantitative pull-off strength, another substrate, a thicker or textured coating, or a different failure mechanism, select and qualify the appropriate method rather than forcing the result into a cross-cut class.