# PVDF architectural coatings

PVDF resin content, factory-applied architectural coating systems, qualification scope and the limits of field repair.

Reviewed: 2026-11-01

Tags: consumables, coatings, pvdf, architectural-finishes

Arkema's **70% Kynar 500** requirement is by **total binder weight**. PPG's **Duranar XL UC139041XL** extrusion example lists **1.90–2.40 mil dry** for primer, color and clearcoat combined, baked **five minutes at 450°F peak metal temperature**. Preserve the individual layer ranges and supplier bake profile for the actual application. [Arkema, licensing and binder-weight requirement](https://kynar500.arkema.com/cms/render/live/en/sites/hpp_kynar500_arkema/home/consistency-through-licensing.html) [PPG, UC139041XL specifications](https://www.ppg.com/en-US/industrialcoatings/product/duranar-xl-extrusion-coating-pueblo/PLP0000020233)

## Resin identity and percentage basis

PVDF is polyvinylidene fluoride. Kynar 500 identifies a resin, while Fluropon and Duranar identify formulated systems. Arkema specifies factory application and bake by a formulator-approved applicator. [Arkema, Kynar 500 specifications](https://kynar500.arkema.com/en/product-information/specifications/)

Arkema’s licensed formulations require at least 70% Kynar 500 by binder weight. In an illustrative **70 kg PVDF + 30 kg other binder** mixture, pigment and application solvent leave that binder ratio unchanged. [Arkema, licensing and binder-weight requirement](https://kynar500.arkema.com/cms/render/live/en/sites/hpp_kynar500_arkema/home/consistency-through-licensing.html)

Sherwin-Williams describes its conventional 70% PVDF blend as having an acrylic remainder. Acrylic selection, pigment durability, solvents and additives also influence the finished coating. Equal PVDF percentages therefore do not make two suppliers’ complete systems interchangeable. PVDF-based architectural products also include powder and other application technologies; obtain the exact product specification rather than transferring a liquid coating’s process to another system. [Sherwin-Williams, PVDF technical white paper, composition](https://industrial.sherwin-williams.com/content/dam/pcg/sherwin-williams/coil-extrusion/emeai/fr/fr-fr/pdfs/general--overview-pdfs/pvdf_fluropon_wp_1.pdf)

## Substrate, preparation and coating construction

The finished system starts below the visible color coat. Cleaning and pretreatment support adhesion and corrosion resistance; the primer connects the prepared metal to the topcoat and must tolerate weathering and, for coil products, subsequent forming. Poor preparation, insufficient film or inappropriate drying can produce blistering or loss of film integrity despite a weather-resistant resin. [Sherwin-Williams, PVDF white paper, film integrity and adhesion](https://industrial.sherwin-williams.com/content/dam/pcg/sherwin-williams/coil-extrusion/emeai/fr/fr-fr/pdfs/general--overview-pdfs/pvdf_fluropon_wp_1.pdf)

Use the specified preparation for the actual aluminium alloy or coated-steel substrate. As one applicator example, Linetec describes an aluminium sequence of cleaning/etching/desmutting, rinsing, chromium-phosphate conversion treatment, further rinsing and drying. That documented line is not a universal recipe or a requirement to use the same chemistry everywhere. Retain the coating supplier’s approved pretreatment sequence and process controls for the selected system. [Linetec, paint process](https://linetec.com/paint/process/)

The number of coats is product-dependent. A primer and color coat form a two-coat system; a clear or barrier layer may be needed for a particular appearance or protection requirement. For example, Sherwin-Williams’ **Fluropon coil data sheet, document SW-CC-2001-9-2018**, lists standard Fluropon as two-coat and Fluropon Classic as an aluminium-pigmented three-coat system with clearcoat. Its standard Fluropon table gives 0.2–0.3 mil primer and 0.7–0.8 mil topcoat, totaling 0.9–1.1 mil. Those values belong to that coil system, not every PVDF finish. [Fluropon coil data sheet](https://industrial.sherwin-williams.com/content/dam/pcg/sherwin-williams/coil-extrusion/na/us/en-us/pdfs/coil-pdfs/fluropon_coil_pds_1.pdf)

## Application and bake: a named extrusion example

Factory application must reach recesses and other required visible surfaces as well as broad faces. Linetec uses electrostatic rotary atomizers and manual reinforcement for difficult geometry, then flash-off and oven processing. Its process description distinguishes **metal temperature** from oven settings and notes the effect of section thickness on heating. A display reading at the oven is insufficient evidence of the part’s bake history. [Linetec, application and curing](https://linetec.com/paint/process/)

PPG’s current **Duranar XL Extrusion Coating – Pueblo, UC139041XL** product page provides a bounded example:

| Item | Published product-specific value |
| --- | --- |
| Construction | Primer, color coat and clearcoat; the family can include an additional barrier coat |
| Primer | UC51742, 0.20–0.30 mil dry |
| Color film | 1.20–1.40 mil dry |
| Clearcoat | UC51132, 0.50–0.70 mil dry |
| Total system | 1.90–2.40 mil dry |
| Bake | Five minutes at 450°F peak metal temperature |

The layer endpoints add to **1.90–2.40 mil**, about **48–61 µm** at 25.4 µm/mil. Keep each layer within its own range and use the supplier’s bake profile for the actual process. [PPG, UC139041XL specifications](https://www.ppg.com/en-US/industrialcoatings/product/duranar-xl-extrusion-coating-pueblo/PLP0000020233)

## Durability standards and claim boundaries

FGIA released **AAMA 2603-26, 2604-26 and 2605-26** in May 2026. They address architectural organic coatings on aluminium extrusions and panels, with a coil-coating appendix, and represent progressively higher performance categories. The update adds pretreatment conversion-coating guidance. Specify the edition and substrate scope explicitly; a coating described as meeting “AAMA 2605” on an undated product page does not itself establish testing to the 2026 revision. [FGIA, 2026 finishes standards release](https://fgiaonline.org/about/news-and-blogs/fgia-updates-suite-of-finishes-documents-for-aluminum-extrusions-panels/)

Request the formulator’s compliance evidence, product identity, approved applicator and agreed acceptance criteria. Arkema’s guide separates certificates, test reports and manufacturer qualifications, and distinguishes aluminium systems from coil-coated galvanized or zinc-aluminium steel systems covered by AAMA 621. A resin licence, a supplier performance claim and project acceptance are different pieces of evidence. [Arkema, liquid coil and extrusion guide specifications, copyright 2023](https://kynar500.arkema.com/files/live/sites/shared_arkema/files/downloads/HPP/market-brochures/construction/specifications/2023%20-%20Kynar%20500%C2%AE%20FSF%C2%AE%20Liquid%20Coil%20and%20Extrusion%20Coatings%20Guide%20Specifications%20.pdf)

Retain method, substrate, exposure and endpoint when comparing results. The Fluropon sheet distinguishes ASTM B117 results for coated steel from aluminium, and separately reports adhesion, bending and weathering. Do not interpret chamber hours as years of building service, or treat resistance to color change as proof of corrosion resistance. A warranty also needs its own written coverage and exclusions. [Fluropon performance tables](https://industrial.sherwin-williams.com/content/dam/pcg/sherwin-williams/coil-extrusion/na/us/en-us/pdfs/coil-pdfs/fluropon_coil_pds_1.pdf)

## Field repair is a separate coating decision

Identify whether damage requires a small cosmetic touch-up, a repair to exposed metal or broader restoration. Linetec warns that its ordinary touch-up products have lower adhesion and durability than factory coatings and should be used sparingly. Its dedicated air-dry fluoropolymer systems are a separate repair/restoration option. Do not assume a color-matched aerosol reproduces the original factory system. [Linetec, touch-up and air-dry systems](https://linetec.com/paint/touch-up/)

PPG’s **Duranar ADS FAQ, footer 01/24, PPG155**, describes a one-component, solvent-based air-dry fluoropolymer repair coating. Bare metal and some other repair conditions require primer. The FAQ distinguishes small artist-brush/pen work from conventional air spray for larger repairs, and states **no warranty for Duranar ADS**. Select the repair process with the coating supplier, including preparation, adhesion, appearance and warranty implications; use the exact current application guide and SDS rather than the factory bake instructions. [PPG Duranar ADS FAQ](https://assets-eu-01.kc-usercontent.com/cce44467-0106-013b-6c0b-26132a361492/70b456df-bb00-40ae-a799-c3dd3aadfffc/Duranar%20ADS%20FAQ_v6%2001-30-24%20HiRes%20%281%29.pdf)

## Related reference

[Surface-finishing processes](../../processes/finishing/index.md)