# Anaerobic threadlockers

Cure conditions, strength and torque test interpretation, fastener selection, assembly and removal, and bounded LOCTITE 243 and Permabond A130 examples.

Reviewed: 2026-11-01

Tags: consumables, adhesives, fasteners, threadlocking

Henkel **LOCTITE 243** lists **22 N·m unseated breakaway** and **9 N·m unseated prevailing torque at 180°** under **ISO 10964**, after **24 hours at 23°C** on **M10 black-oxide bolts and mild-steel nuts**. These are removal-test values. Establish tightening torque and clamp load with the actual fastener finish, adhesive and assembly procedure. [Henkel, *LOCTITE 243 TDS*, pp. 2, 4](https://datasheets.tdx.henkel.com/LOCTITE-243-en_GL.pdf)

## Function and cure mechanism

Threadlockers cure in confined metal threads as oxygen is excluded and active metal ions are available. Use the grade for the joint and application method. [Permabond, *Anaerobic Adhesives & Sealants*](https://permabond.com/products/anaerobic-adhesives-and-sealants/)

The cured adhesive resists loosening and seals thread clearances. Product families vary in viscosity, gap capability, temperature resistance, strength, and removability. Low-viscosity wicking grades can be intended for post-assembly application, whereas other grades are applied before assembly. Choose the application method with the grade rather than assuming any liquid threadlocker will penetrate an assembled joint. [Permabond, threadlocker overview](https://permabond.com/products/anaerobic-adhesives-and-sealants/).

## Metal, clearance, contamination, and activator

Cure depends on the actual surface. Permabond A130's TDS states that copper and its alloys accelerate cure, while oxidized or passivated surfaces such as stainless steel slow it. Lower temperature and larger gaps also extend cure time. Its maximum gap-fill value is 0.12 mm and maximum thread size M20; neither value authorizes repair of damaged threads. [Permabond, *A130 TDS*, revision 6, December 11, 2025](https://permabond.com/tds/a130_tds-en/?pdf=1).

Oil tolerance is product-specific. Henkel describes LOCTITE 243 as curing through most light corrosion-prevention oils and cutting-fluid coatings on as-received fasteners, but recommends cleaning heavily oiled or contaminated parts. Passive metals and low temperature can still require activation when cure is too slow. “Oil tolerant” therefore does not mean arbitrary grease, residue, cleaner, or contamination is acceptable. [Henkel, *LOCTITE 243*, preparation instructions](https://next.henkel-adhesives.com/us/en/products/industrial-adhesives/central-pdp.html/loctite-243/BP000000316211/variation/1330906.html).

An activator supplies a different process condition. Permabond's A905 instructions call for clean, dry, grease-free surfaces, application to one component, solvent evaporation, and adhesive application to the untreated second component. **Do not mix A905 directly into the adhesive.** Its TDS says it can accelerate cure and extend usable gap capability, but compatibility and cure remain dependent on the selected substrates and adhesive. Activation is not a universal substitute for cleaning or proof that an otherwise unsuitable joint will work. [Permabond, *A905 TDS*, revision 3](https://permabond.com/tds/a905_tds-en/?pdf=1).

## Strength grades and torque measurements

Low-, medium-, and high-strength labels describe a product's intended behavior, not an installation torque. Color is also insufficient identification. For example, Permabond lists red A011 as low strength and easy to remove, while other red products are high-strength or permanent grades. Preserve manufacturer, full product designation, and applicable data sheet. [Permabond, *Anaerobic Product Selector Guide*](https://permabond.com/products/anaerobic-adhesives-and-sealants-selector-guide/).

**Breakaway torque** concerns initiation of rotation after cure; **prevailing torque** concerns continued rotation after the initial bond break. Henkel's manual distinguishes tests of unseated fasteners from pre-torqued assemblies and treats the test method and specimen as part of the result. Thread diameter, finish, engagement, cure, temperature, and initial tightening condition matter when comparing values. A table entry without those conditions is incomplete engineering data. [Henkel, *How to Increase Reliability and Prevent Threaded Assembly Failure*, testing appendix](https://dm.henkel-dam.com/is/content/henkel/LOCTITE-Threadlocker-Manual).

### Named example: LOCTITE 243

The **April 2025 TDS** reports the following typical ISO 10964 results after 24 hours at 23°C, using **M10 black-oxide bolts and mild-steel nuts**:

| Test condition | Reported torque |
| --- | --- |
| Unseated, breakaway | 22 N·m |
| Unseated, prevail at 180° | 9 N·m |

Check removal behavior on the actual joint. Use the tightening process specified below for assembly. [Henkel, *LOCTITE 243 TDS*, pp. 2, 4](https://datasheets.tdx.henkel.com/LOCTITE-243-en_GL.pdf)

## Installation torque and cure milestones

Threadlocker does not replace the joint's preload design. Henkel's manual relates tightening torque to clamp force through friction and geometry; the empirical K-factor depends on materials and assembly conditions. Changing from dry threads to a liquid-treated condition can change the torque-to-tension relationship. Use a joint-specific tightening process qualified for the actual fastener finish and adhesive rather than subtracting published removal torque or applying a universal percentage correction. [Henkel, threaded assemblies and torque–tension discussion](https://dm.henkel-dam.com/is/content/henkel/LOCTITE-Threadlocker-Manual).

**Handling or fixture strength is not full cure.** A130's M10-steel data at 23°C give 15 minutes to handling, 1 hour to working strength, and 24 hours to full strength. Its instructions require adhesive across the thread contact length for through holes and down the internal threads for blind holes, followed by assembly and tightening. Excess outside the confined joint remains uncured in air; its liquid appearance does not establish failure of the adhesive inside. These times and observations apply to that product and context. [Permabond, *A130 TDS*](https://permabond.com/tds/a130_tds-en/?pdf=1).

## Temperature, fluids, and disassembly

Henkel's 243 TDS distinguishes hot strength from fluid-exposure results measured afterward at 23°C. Retain the fluid, concentration, exposure temperature, and duration with each claim. It excludes oxygen-rich systems and strong oxidizers, and cautions about thermoplastic stress cracking. [Henkel, *LOCTITE 243 TDS*, environmental resistance and general information](https://datasheets.tdx.henkel.com/LOCTITE-243-en_GL.pdf).

For 243 removal, Henkel specifies hand tools, or localized heat around 250°C for unusually long engagement, followed by disassembly while hot. This is not a service-temperature rating. Engineering synthesis: assess surrounding components and fastener temperature limits before heating. [Henkel, *LOCTITE 243 TDS*, disassembly](https://datasheets.tdx.henkel.com/LOCTITE-243-en_GL.pdf).

## Product-specific handling and selection record

The GB SDS retrieved for **LOCTITE 243, material 1335884**, is SDS 817149, **V004.0, revised June 11, 2026**. It classifies the supplied mixture as a skin sensitizer and chronically harmful to aquatic life, directs protective-glove use, and calls for avoiding environmental release. This is a specific regional formulation record; it must not be replaced by an old “243” SDS or transferred automatically to another supplier or country. Use the supplied product's current regional SDS for handling. [Henkel, *LOCTITE 243 GB SDS*, §§1–2](https://api.henkeldx.com/v1/mysds/SafetyDataSheetSet?Appid=%27YPSSW_SDSUA_EXT%27&Dmskey=%27%27&Laiso=%27EN%27&Matnr=%271335884%27&Rvlid=%27GB%27).