# Nickel-acetate sealing formulations

Supplied nickel-acetate anodizing seals, exact-product ingredient disclosures, quantity bases, reference properties, and limits of sealing-quality evidence.

Reviewed: 2026-10-30

Tags: chemicals, anodizing, surface-finishing

## Identity and boundaries

The **Specialty Sealant powder** SDS lists **50–75 wt% nickel acetate tetrahydrate** (CAS 6018-89-9). The **Specialty Sealant MTL liquid** SDS lists **5–10 wt% nickel(II) acetate** (CAS 373-02-4). These are salt disclosures for the supplied products. Working-bath elemental nickel requires separate evidence. [Powder SDS][seal-sds] [MTL SDS][mtl-sds] The powder TDS names dyed, clear, hardcoat and electrolytically colored anodize. [Specialty Sealant TDS, revised 26 July 2023][seal-tds]

The supplier also lists High Purity Nickel Acetate used with a wetting agent and Specialty Dispersant for controlling sealing smut. These have separate product identities. [Nickel Acetate TDS, revised 11 July 2019][nickel-tds] [Specialty Dispersant TDS, revised 13 October 2022][dispersant]

SurTec's portfolio separately identifies nickel-fluoride cold seals, nickel-free dye fixation, nickel-free mid-temperature seals, and hot-water sealing products. SurTec 351 Hardwall dye fixation has a subsequent seal recommendation. SurTec 650 is described separately as passivation for anodized surfaces. **Synthesis.** Dye, dye fixation, cold seal, nickel-acetate seal, and conversion or passivation chemistry are not interchangeable identities. "Nickel-containing" alone does not identify the counterion or the process class. [SurTec anodizing portfolio][surtec]

## Exact supplied products and ingredient disclosures

The following historical U.S. supplier SDS documents identify products by name, without a separate part number or grade. The percentages are ingredient mass divided by total supplied-product mass, multiplied by 100. They are neither elemental-nickel assays nor working-bath concentrations. Both sheets withhold specific identities or exact percentages as trade secrets.

| Product and SDS version | Complete section 3 ingredient list, weight % | Identity limits |
| --- | --- | --- |
| Specialty Sealant, version 3, 26 May 2021 | Nickel acetate tetrahydrate, CAS 6018-89-9, 50–75%; proprietary surfactant, 25–50%; benzoic acid, CAS 65-85-0, 1.0–25% | Green powder. Ranges are disclosures, not a nominal formula. [SDS, sections 1, 3, and 9][seal-sds] |
| Specialty Sealant MTL, version 4, 20 May 2021 | Nickel(II) acetate, CAS 373-02-4, 5–10%; acetic acid, CAS 64-19-7, 1.0–5%; nonylphenol, ethoxylated, CAS 127087-87-0, 1.0–5%; proprietary surfactant, 1.0–10% | Green liquid. The nickel entry uses a different CAS identity from the powder's tetrahydrate. [SDS, sections 1, 3, and 9][mtl-sds] |

The notes mark health or environmental hazards, workplace exposure limits, and, for the MTL ethoxylated nonylphenol entry, PBT or vPvB status. MTL's proprietary surfactant row says "Not Classified" while carrying the hazard-note marker. That inconsistency is not resolved into a new classification here. [Powder SDS, p. 2][seal-sds], [MTL SDS, p. 3][mtl-sds]

OSHA's section 3 requirements concern hazard-relevant ingredients and permit concentration ranges in specified circumstances. **Synthesis.** Such disclosure does not necessarily account for every constituent. The powder's upper bounds cannot all be actual simultaneous mass fractions because their sum exceeds 100%. Normalizing the ranges to 100% would invent a formulation. An unlisted ingredient is not demonstrated absent. [OSHA SDS Appendix D, section 3][osha]

## Functions and performance claims

Specialty Sealant's TDS describes pH regulation and a smut suppressant. It claims compatibility with all aluminum dyes and corrosion protection, but supplies no dye-by-dye results, numerical corrosion dataset, alloy matrix, or exposure endpoint. It lists ASTM B136, B680, and B117 without editions. Those statements remain manufacturer claims within the sheet's application context, not current-lot certification. The 2023 TDS and 2021 SDS are different document revisions and do not establish unchanged composition between dates. [Specialty Sealant TDS][seal-tds]

Specialty Dispersant's claimed smut-free behavior depends on preceding anodizing conditions stated in its sheet. The claim is therefore not unconditional. The sheet supplies no analytical method for dispersant concentration control. [Specialty Dispersant TDS][dispersant]

**Synthesis.** A disclosed surfactant supports identifying a surface-active ingredient class, not a universal surfactant identity or a guaranteed low-bloom result. The powder's pH-regulation claim does not identify which ingredient provides that function. The cited disclosures do not establish a complexant package, a common buffer system across brands, or universal presence of benzoic acid. No quantified dye-bleed result, low-bloom test, or standardized anti-smut rating was verified for these products.

## Reference properties and measurement bases

These are supplied-product SDS entries, not bath targets or process settings.

| Property | Specialty Sealant powder | Specialty Sealant MTL liquid |
| --- | --- | --- |
| Appearance and odor | Green powder; acetic-acid odor | Green liquid; mild acetic-acid odor |
| pH | Not measured | 5.0–5.8; sample preparation and test temperature unspecified |
| Specific gravity | Not measured | 1.06–1.09; sample and reference temperatures unspecified |
| Water solubility | Not measured | Described as complete; test temperature and quantitative basis unspecified |
| Total solids or active content | No assay reported | No assay reported |

Sources are [Specialty Sealant SDS, section 9, pp. 5–6][seal-sds] and [MTL SDS, section 9, pp. 6–7][mtl-sds]. The MTL sheet gives no dilution basis for pH. Its location in the product-property section does not establish a standardized neat-sample method. Specific gravity is dimensionless, not a density in g/mL. Neither specific gravity nor complete solubility measures solids or active strength.

The following quantity distinctions are explanatory synthesis.

- Salt mass includes nickel, acetate, and any water of crystallization. Tetrahydrate mass and anhydrous-salt mass are different reporting bases. Elemental nickel excludes acetate and hydration water. Acetate content is another numerator, distinct from separately disclosed acetic acid.
- Ingredient weight percent concerns the supplied mixture. Product mass per bath volume and dissolved nickel per bath volume concern a different sample. A percent by volume has a volume denominator and cannot replace a mass percent without additional physical data.
- A dry-powder property, a prepared test-solution property, and a measured bath property describe different material states. Product pH does not establish actual bath pH.
- Nickel retained in a treated film, expressed per film mass or coated area, has another denominator. No deposited-film assay or retention fraction follows from the ingredient table.

A raw-material example illustrates the distinction. A.M.P.E.R.E.'s undated tetrahydrate sheet identifies CAS 6018-89-9 and a minimum nickel content of 23%. That is the supplier's raw-material nickel specification, not the nickel percentage of either formulated seal above. The sheet does not specify the assay method or a current lot result. [A.M.P.E.R.E. nickel acetate][ampere]

## Sealing quality is a coating measurement

Public publisher scopes distinguish tests of the treated coating. They do not make concentrate composition proof of complete sealing or a completed ageing state.

| Public edition | Measurement and applicability limits |
| --- | --- |
| ISO 2143:2017, edition 3 | Dye absorption after acid pretreatment estimates loss of absorptive power. Excludes deep shades, coatings below 3 µm, dichromate seals, supplementary oiling, waxing, or lacquering, and alloys above 2% copper or 4% silicon. The scope says it is less appropriate for hydrothermal seals with nickel salts, cobalt salts, or organic additives. [ISO public scope][iso-dye] |
| ISO 2931:2017, edition 4 | Admittance assessment applies to aqueous seals. Different sealing methods need not yield comparable results. Comparisons also have alloy limits above 2% silicon, 5% manganese, or 3% magnesium. The scope requires sufficient area and thickness above 3 µm. Acceptance use depends on anodizer-customer agreement. [ISO public scope][iso-admittance] |
| ISO 3210:2025, edition 5 | Destructive mass-loss assessment distinguishes phosphoric-acid-based methods with and without prior acid treatment. Excludes normally unsealed hard-type coatings, dichromate-only seals, chromic-acid anodizing, and hydrophobic treatments. The publisher lists the 2017 edition as withdrawn. [ISO public scope][iso-mass] |

These are scope summaries, without test procedures or paid acceptance tables. An older supplier's editionless ASTM references do not establish results under the ISO editions above. Appearance, smut suppression, dye retention, and corrosion resistance are different outcomes. None substitutes for an applicable coating test with its specimen and treatment history.

## Source coverage and limits

Reviewed on 30 October 2026 PDT. Coverage includes the complete two-page Specialty Sealant and Nickel Acetate technical sheets, the complete one-page Specialty Dispersant sheet, both complete SDS documents, and their ingredient notes and product-property tables. The SDS evidence is historical and U.S.-oriented. Current regional formulations, current lots, complete proprietary compositions, and a matching MTL technical sheet remain unverified.

Indexed ANODAL Seal AS Liquid and Bright Dyes MT-90 technical sheets were not retrievable as the expected documents. Their cached numerical and performance claims are not adopted. The SurTec and A.M.P.E.R.E. pages are undated retrieval snapshots, not formulation revisions. Only public standards descriptions were used.

**Synthesis.** Free-of claims need a defined substance scope and analytical detection basis before they can mean zero measured content. No nickel-free, fluoride-free, cobalt-free, or chromium-free assay is established for the compared nickel-acetate products. Supplier compliance language does not establish medical, food-contact, aerospace, customer, wastewater, or general environmental approval. This evidence supplies no mixing formula, bath preparation, operating recipe, replenishment rule, or customer capability.

## Related references

[Nickel acetate substance](../substances/nickel-acetate.md), [cold-seal formulations](anodizing-cold-seal-formulations.md), [anodizing dyes](anodizing-dyes.md), and [Surface-finishing processes](../../processes/finishing/index.md) cover adjacent subjects. These related articles remain unpublished in the source catalog at this review date.

[seal-tds]: https://www.usspecialty.com/tds/Sealant.pdf
[nickel-tds]: https://www.usspecialty.com/tds/NickelAcetate.pdf
[dispersant]: https://www.usspecialty.com/tds/Dispersant.pdf
[seal-sds]: https://www.usspecialty.com/sds/SpecialtySealant-SDS.pdf
[mtl-sds]: https://www.usspecialty.com/sds/SpecialtySealantMTL-SDS.pdf
[surtec]: https://www.surtec.com/en/applications/metal-pre-treatment/anodizing-portfolio/
[osha]: https://www.osha.gov/laws-regs/regulations/standardnumber/1910/1910.1200AppD
[ampere]: https://www.ampere.com/en/cproduct/nickel-acetate/
[iso-dye]: https://www.iso.org/standard/70154.html
[iso-admittance]: https://www.iso.org/standard/70155.html
[iso-mass]: https://www.iso.org/standard/88866.html