## Identity and construction

Klingspor **CS 561 item 11016** lists **125 × 22 mm**, a **star-shaped opening**, grain **80** and maxima of **80 m/s** and **12,200 rpm**. The 22 mm opening describes the disc, while the spindle thread and pad have separate fit requirements. [CS 561 UK sheet](https://www.klingspor.co.uk/products/fibre-discs/cs-561/pdf) The disc carries grain and resin on one face of vulcanized fiber. [Klingspor fiber-disc reference](https://www.klingspor.de/en/lowdown-on-grinding/fibre-disc)

Klingspor makes vulcanized fiber by parchmentizing cellulose or cotton webs without added bond between those webs. Its **0.38–0.84 mm** range describes common backing thickness. Exact disc thickness requires item data. [Klingspor vulcanized-fiber definition](https://www.klingspor.de/en/lowdown-on-grinding/vulcanised-fibre)

The maker coat attaches abrasive grain to the backing. The later size coat anchors the grain further. Klingspor calls the latter top binding and describes its support against lateral grinding forces. An additional grinding-active layer, such as VSM TOP SIZE, is a separate construction attribute. A resin-bonded label does not disclose the individual coating weights or full resin formulation. [Klingspor coated-abrasive components](https://www.klingspor.com/coated-abrasives-basics), [top binding](https://www.klingspor.de/en/lowdown-on-grinding/top-bonding), [VSM XF870 sheet](https://www.us.vsmabrasives.com/en/xf870?file=files/content/PDS/2024+VSM-Product-Data-Sheet-XF870-EN.pdf.pdf)

## Related disc constructions

| Construction | Distinction from a vulcanized-fiber coated disc |
| --- | --- |
| Fiberglass-reinforced bonded grinding wheel | Abrasive, resin, and fillers form the wheel body, with glass-fiber reinforcing layers. Glass fiber is reinforcement rather than the cellulose sheet carrying a face coating. [Klingspor Kronenflex construction](https://www.klingspor.de/en/products/anwendung/kronenflex-trennscheiben) |
| Flap disc, also called abrasive mop disc | Abrasive-coated cloth flaps are arranged on a backing plate. Klingspor's SMT plates include glass fiber and glass-fiber-reinforced plastic. A fiberglass plate does not make the flaps a vulcanized-fiber disc. [Klingspor flap-disc construction](https://www.klingspor.de/en/products/vorteile/schleifmopteller) |
| Nonwoven abrasive disc | Grain and resin occupy an open three-dimensional web of nylon fibers. The web differs from a face-coated sheet. [Klingspor NWT construction](https://www.klingspor.com/shop/nwtcrse-s6x9-187557) |
| Paper or cloth coated disc | The carrier is paper or textile rather than the dense vulcanized-fiber backing. A common grain or disc shape does not establish the same backing. [Klingspor backing categories](https://www.klingspor.com/coated-abrasives-basics) |
| Disc, pad, retaining hardware, and machine assembly | Fit and operating restrictions depend on the components together. The abrasive disc alone is not a complete qualified assembly. [FEPA fiber-disc leaflet](https://fepa-abrasives.org/wp-content/uploads/2020/04/fepa-safety-leaflet-fibre-discs-english.pdf) |

## Sampled supplier products

These examples compare stated construction. They are neither interchangeable products nor a ranking of grain technologies.

| Product | Stated construction | Bounded product information |
| --- | --- | --- |
| [Klingspor CS 561, UK sheet](https://www.klingspor.co.uk/products/fibre-discs/cs-561/pdf) | Aluminum oxide, resin bond, close coat. Klingspor identifies vulcanized fiber as the backing for this family in its fiber-disc reference. | Catalog 11016 is 125 × 22 mm, star-shaped hole, grain 80, 80 m/s maximum, 12,200 rpm maximum. The sheet also has round-hole and X-LOCK variants. |
| [VSM XF870, US sheet P/XF870/04.WW/8.24/en/1](https://www.us.vsmabrasives.com/en/xf870?file=files/content/PDS/2024+VSM-Product-Data-Sheet-XF870-EN.pdf.pdf) | Ceramic grain, full-resin bond, vulcanized fiber, medium coat, and additional TOP SIZE layer. | Identifies medium pressure and processing stainless steel and superalloys. Filled grit boxes identify 24, 36, 40, 50, 60, 80, 100, and 120. Other printed numbers have unfilled boxes. |
| [3M Cubitron II 982C, item 7000119200](https://www.3m.com/3M/en_US/p/d/v000145575/) | Precision-shaped ceramic grain, stiff fiber backing, strong resin bond. | The item is 80+, 5 in × 7/8 in, Die 500P, center-hole attachment. The page describes carbon-steel grinding. Its backing description alone does not disclose backing thickness or cellulose composition. |

VSM's 58 in production width is not a finished-disc diameter. Its grain-fracture diagram has no numerical time axis. The footnote permits further grit sizes on request and reserves technical changes. [VSM XF870, complete sheet and diagram](https://www.us.vsmabrasives.com/en/xf870?file=files/content/PDS/2024+VSM-Product-Data-Sheet-XF870-EN.pdf.pdf)

## Grain designation and dimensional quantities

Grain size is a distribution, not a single particle diameter. FEPA P denotes coated-abrasive grading, whereas FEPA F has a different scope. ANSI coated, ANSI bonded, and proprietary classifications also need their own identities. UAMA's explanation cites historical editions, including ANSI B74.18-1996, and does not certify current product grades. [UAMA grading and measurement reference](https://uama.org/abrasives-101/)

The unprefixed 80 on the sampled Klingspor and VSM sheets and 3M's 80+ remain as printed. Neither the shared number nor the word ceramic establishes equal particle distributions, cutting behavior, or finish. **Synthesis.** Grain grading, grain shape, backing support, and grinding conditions describe different influences. A grade number alone supplies no universal micron conversion or surface-roughness value. [UAMA particle-size and performance discussion](https://uama.org/abrasives-101/), [3M exact item](https://www.3m.com/3M/en_US/p/d/v000145575/)

| Quantity | Meaning and boundary |
| --- | --- |
| Disc diameter and bore, mm or in | Overall disc size and center-opening size. Hole shape, slots, and attachment system remain separate attributes. |
| Backing thickness, mm | Thickness of the fiber carrier, distinct from grain grade and total coated thickness. |
| Pad diameter and contact geometry | Supporting component dimensions and face form. Hardness descriptions such as flexible or hard are supplier categories, not a universal numerical scale. |
| Spindle thread and retaining hardware | Machine connection and clamping arrangement. A 22 mm disc opening is not an M14 thread. |
| Rotational speed, rpm or min⁻¹ | Revolutions per minute. This is distinct from peripheral speed in m/s. |

**Synthesis.** These distinctions follow the separate fields in the disc and pad sheets and FEPA's mounting illustrations. Matching nominal diameter or bore leaves the thread, retaining nut or flange, clearance, guard, and permissible combination unresolved. [CS 561 sheet](https://www.klingspor.co.uk/products/fibre-discs/cs-561/pdf), [ST 358 A sheet](https://www.klingspor.de/en/products/backing-pads/st-358-a/pdf), [FEPA leaflet, both pages](https://fepa-abrasives.org/wp-content/uploads/2020/04/fepa-safety-leaflet-fibre-discs-english.pdf)

## Backing pads and speed limits

Klingspor distinguishes the smooth, flexible ST 358 pad from its hard, ribbed ST 358 A. The ST 358 A webpage identifies a retaining nut and separate M14, 5/8-inch, and X-LOCK versions. These are product variants, not a universal grinder connection. [Klingspor fiber-disc and pad relationships](https://www.klingspor.de/en/lowdown-on-grinding/fibre-disc), [ST 358 A webpage](https://www.klingspor.de/en/products/backing-pads/st-358-a)

The German and South African ST 358 A downloads list catalog 126347 as a 125 mm M14 pad for 125 × 22 mm discs, rated 80 m/s and 12,250 rpm. The sampled CS 561 125 mm disc lists 12,200 rpm independently. A pad's higher printed value does not raise a disc's limit. Neither pad download supplies a revision date. [German ST 358 A sheet](https://www.klingspor.de/en/products/backing-pads/st-358-a/pdf), [South African ST 358 A sheet](https://www.klingspor.co.za/products/backing-pads/st-358-a/pdf), [CS 561 sheet](https://www.klingspor.co.uk/products/fibre-discs/cs-561/pdf)

For circular geometry, peripheral speed is `v = π × D × n / 60`, with diameter `D` in meters, rotational speed `n` in rpm, and `v` in m/s. **Derived example.** At nominal 125 mm and 12,200 rpm, the calculated rim speed is about 79.8 m/s. This arithmetic describes geometry only. It cannot rate an unidentified disc, round a marked limit upward, qualify an assembly, or establish a suitable grinding setting.

FEPA's 2017 leaflet covers coated fiber discs on angle grinders. Its diagrams address the backing pad, retaining-nut orientation, guards, damage, and marked speeds. It prohibits cutting with these grinding discs. Maximum ratings bound use. They do not establish an optimum speed, pressure, contact angle, or heat input for a particular workpiece. The leaflet does not qualify an individual assembly. [FEPA leaflet, marking panel and eleven illustrated recommendations](https://fepa-abrasives.org/wp-content/uploads/2020/04/fepa-safety-leaflet-fibre-discs-english.pdf)

## Moisture, chemistry, and application limits

Klingspor describes its fiber backing as not waterproof. VSM's sampled XF870 sheet carries a crossed-out wet-grinding pictogram. Neither a ceramic grain nor a resin bond establishes wet-use suitability for other finished discs, their pads, or their machines. [Klingspor backing discussion](https://www.klingspor.com/coated-abrasives-basics), [XF870 sheet pictograms](https://www.us.vsmabrasives.com/en/xf870?file=files/content/PDS/2024+VSM-Product-Data-Sheet-XF870-EN.pdf.pdf)

Cellulose exchanges moisture with its surroundings. Klingspor associates humidity extremes with disc buckling and recommends approximately 45–65% relative humidity. It also associates local overheating with backing blisters and grain shedding. These are Klingspor material and storage statements, not storage qualification for all suppliers. The 3M SDS instead states no special storage requirements. [Klingspor vulcanized-fiber reference](https://www.klingspor.de/en/lowdown-on-grinding/vulcanised-fibre), [3M 982C SDS, section 7](https://cdmsweb.3m.com/ingredientcommunication/file/Media/clKTpshf2pE=)

The US 3M 982C family SDS, document 26-6645-1, version 4.00, issued December 17, 2024, covers 36+, 60+, 80+, and several attachment forms. Section 3 reports 40–75% fiber backing, 10–30% ceramic aluminum oxide mineral, 5–15% inorganic fluoride, 3–15% cured resin, less than 7% steel or plastic attachment, and 1–5% filler by weight. These family ranges are whole-product composition, not abrasive purity, coated area, residue transfer, or a complete lot formulation. [3M SDS, sections 1–3](https://cdmsweb.3m.com/ingredientcommunication/file/Media/clKTpshf2pE=)

That SDS also identifies workpiece-generated combustible dust and hydrogen fluoride from extreme overheating. Its product classification does not characterize every grinding exposure. **Synthesis.** Supplier substrate listings and grinding-aid claims do not prove absence of transferred residue or suitability for later welding, coating, bonding, or corrosion-sensitive service. No residue or downstream-compatibility tests were reviewed here. [3M SDS, sections 7–11](https://cdmsweb.3m.com/ingredientcommunication/file/Media/clKTpshf2pE=)

## Source coverage and uncertainty

Coverage includes the five-page CS 561 stock table, the one-page XF870 sheet with filled grit boxes, wear diagram, pictograms, and footnote, both regional ST 358 A sheets, FEPA's two-page 2017 leaflet, and all nine pages of the US 982C SDS. The 3M product page's visible description and exact-item identity were available, but its full dynamic properties table was not retrieved. Unreported properties remain unknown. The Klingspor pages and downloads are undated snapshots.

Manufacturer statements about longer life, cooler grinding, or greater removal lack a complete matched test protocol in these sampled product documents. They supply no transferable life multiplier, removal rate, finish guarantee, safe contact force, or production recipe. [VSM XF870 claims and diagram](https://www.us.vsmabrasives.com/en/xf870?file=files/content/PDS/2024+VSM-Product-Data-Sheet-XF870-EN.pdf.pdf), [3M 982C product claims](https://www.3m.com/3M/en_US/p/d/v000145575/)

Full normative standards, machine manuals, every disc variant, and independent compatibility testing are outside this coverage. Public labels and safety guidance do not establish complete-assembly conformity or customer capability.

## Related references